Allgemein
Mechanisch
Property | Temperature | Value |
---|---|---|
Biegefestigkeit | 23.0 °C | 25.5 MPa Show Supplier Material materials with Biegefestigkeit of 25.5 MPa |
Biegefestigkeit, transversal | 23.0 °C | 20 MPa Show Supplier Material materials with Biegefestigkeit, transversal of 20 MPa |
Druckfestigkeit | 23.0 °C | 59 MPa Show Supplier Material materials with Druckfestigkeit of 59 MPa |
Druckfestigkeit, transversal | 23.0 °C | 59 MPa Show Supplier Material materials with Druckfestigkeit, transversal of 59 MPa |
Elastizitätsmodul | 23.0 °C | 11 GPa Show Supplier Material materials with Elastizitätsmodul of 11 GPa |
Elastizitätsmodul, transversal | 23.0 °C | 9.3 GPa Show Supplier Material materials with Elastizitätsmodul, transversal of 9.3 GPa |
Hardness, Rockwell R | 23.0 °C | 95 [-] Show Supplier Material materials with Hardness, Rockwell R of 95 [-] |
Zugfestigkeit | 23.0 °C | 19 MPa Show Supplier Material materials with Zugfestigkeit of 19 MPa |
Zugfestigkeit, transversal | 23.0 °C | 15 MPa Show Supplier Material materials with Zugfestigkeit, transversal of 15 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Aschegehalt | 23.0 °C | 0.15 % Show Supplier Material materials with Aschegehalt of 0.15 % | |
Koeffizient der thermischen Ausdehnung | 23.0 °C | 3E-6 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 3E-6 1/K | average for 20-100°C |
Thermal conductivity, in-plane | 23.0 °C | 170 W/(m·K) Show Supplier Material materials with Thermal conductivity, in-plane of 170 W/(m·K) | |
Thermal conductivity, through-plane | 23.0 °C | 150 W/(m·K) Show Supplier Material materials with Thermal conductivity, through-plane of 150 W/(m·K) | |
thermischer Ausdehnungskoeffizient, transversal | 23.0 °C | 3.7E-6 1/K Show Supplier Material materials with thermischer Ausdehnungskoeffizient, transversal of 3.7E-6 1/K | average for 20-100°C |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 23.0 °C | 7E-6 Ω·m Show Supplier Material materials with spezifischer Widerstand of 7E-6 Ω·m |
spezifischer Widerstand, transversal | 23.0 °C | 7.5E-6 Ω·m Show Supplier Material materials with spezifischer Widerstand, transversal of 7.5E-6 Ω·m |
Technological properties
Property | ||
---|---|---|
Application areas | CZ silicon crystal growth, Quartz processing, Purified electronic fixturing, Polysilicon seed chucks |