Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 2.72 g/cm³ Show Supplier Material materials with Dichte of 2.72 g/cm³ |
Abmessung
Property | Value |
---|---|
Dicke | 0.06 - 1 mm Show Supplier Material materials with Dicke of 0.06 - 1 mm |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung A50 | 23.0 °C | 1 % Show Supplier Material materials with Dehnung A50 of 1 % |
Streckgrenze | 23.0 °C | 155 MPa Show Supplier Material materials with Streckgrenze of 155 MPa |
Zugfestigkeit | 23.0 °C | 170 - 175 MPa Show Supplier Material materials with Zugfestigkeit of 170 - 175 MPa |
Thermisch
Property | Temperature | Value |
---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 2.4E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 2.4E-5 1/K |
Chemical properties
Property | Value |
---|---|
Eisen | 0.7 - 1.3 % Show Supplier Material materials with Eisen of 0.7 - 1.3 % |
Kupfer | 0.05 % Show Supplier Material materials with Kupfer of 0.05 % |
Silizium | 0.05 - 0.3 % Show Supplier Material materials with Silizium of 0.05 - 0.3 % |
Zink | 0.1 % Show Supplier Material materials with Zink of 0.1 % |
Technological properties
Property | ||
---|---|---|
Application areas | Roofing: Foil for bituminous coating; Heat exchangers: Fins, Heat exchangers; Insulation; Semi-rigid and corrugated: Pet food; Foil stock: Foil app; Components: Automotive fins, Heat exchangers | |
Corrosion properties | Moderated | |
Workability | Excellent |