Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 1.3 g/cm³ Show Supplier Material materials with Dichte of 1.3 g/cm³ | ISO 1183 |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 85 MPa Show Supplier Material materials with Biegefestigkeit of 85 MPa | ISO 178 (2mm/min) |
Biegemodul | 23.0 °C | 2.6 GPa Show Supplier Material materials with Biegemodul of 2.6 GPa | ISO 178 (2mm/min) |
Dehnung | 23.0 °C | 8 % Show Supplier Material materials with Dehnung of 8 % | ISO 527-2 (5mm/min) |
Elastizitätsmodul | 23.0 °C | 2.7 GPa Show Supplier Material materials with Elastizitätsmodul of 2.7 GPa | ISO 527-2 (1mm/min) |
Schlagfestigkeit, Charpy gekerbt | 23.0 °C | 8 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 8 kJ/m² | ISO 179/1eA |
Schlagzähigkeit, Charpy ungekerbt | 23.0 °C | 75 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 75 kJ/m² | ISO 179/1eU |
Schlagzähigkeit, Izod gekerbt | 23.0 °C | 7 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Izod gekerbt of 7 kJ/m² | ISO 180/1A |
Schlagzähigkeit, Izod ungekerbt | 23.0 °C | 70 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Izod ungekerbt of 70 kJ/m² | ISO 180/1U |
Zugfestigkeit | 23.0 °C | 65 MPa Show Supplier Material materials with Zugfestigkeit of 65 MPa | ISO 527-2 (5mm/min) |
Thermisch
Property | Value | Comment | |
---|---|---|---|
Heat deflection temperature, 0.45 MPa | 160 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 160 °C | ISO 75-2/B | |
Heat deflection temperature, 1.80 MPa | 60 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 60 °C | ISO 75-2/A | |
Schmelzpunkt | 225 °C Show Supplier Material materials with Schmelzpunkt of 225 °C | ISO 3146 | |
Entflammbarkeit | UL94 (0.8mm) HB |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
Kriechstromfestigkeit | 23.0 °C | 600 V Show Supplier Material materials with Kriechstromfestigkeit of 600 V | EN 60112 |
Surface resistivity | 23.0 °C | 1.00E+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1.00E+13 Ω/sq | ASTM D257 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | EPIMIX PBT is used in all sectors of industry, has and excellent surface finish, low warpage and all around excellent mechanical properties. EPIMIX PBT is approved for applications in direct contact with drinking water and food. | |
Certifications | Drinking Water,Food Contact | |
Other | Laboratory conditions are 23 ±2°C and 45-55 % RH. |