A high quality aerospace grade aluminum alloy (6061B) reinforced with 20 vol.% silicon carbide particles which produces a metal matrix composite (MMC). 620XF is manufactured via a powder metallurgy route using a mechanical alloying process to ensure a homogeneous reinforcement distribution, providing a refined grain structure enhancing mechanical properties. The MMC is heat treatable offering high strength and modulus for structural applications and is available in billet, forged and extruded forms.


620XF Advantages:


  • Precision section extrusion using standard dies
  • Reduced wall thickness offering weight saving
  • High stiffness and strength
  • Robust and ductile for damage resistance
  • Good corrosion and fatigue performance
  • Thermally stable
  • Equivalent Materials

    Diese Materialdaten wurden von Materion Brush GmbH zur Verfügung gestellt

    Alle Daten beziehen sich auf Raumtemperatur soweit nicht anderweitig spezifiziert. SI Einheiten werden verwendt soweit nicht anderweitig spezifiziert.
    Äquivalente Standards sind ähnlich zu einem oder mehreren Standards die der Anbieter angegeben hat. Manche äquivalente Standards können strikter sein oder außerhalb der Bedingungen des ursprünglichen Standards.

    Ashby charts

    See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

    Eigenschaften

    Allgemein

    PropertyTemperatureValue

    Dichte

    23.0 °C

    2.8 g/cm³

    Show Supplier Material materials with Dichte of 2.8 g/cm³

    Mechanisch

    PropertyTemperatureValue

    Dehnung

    23.0 °C

    7 %

    Show Supplier Material materials with Dehnung of 7 %

    Elastizitätsmodul

    23.0 °C

    103 GPa

    Show Supplier Material materials with Elastizitätsmodul of 103 GPa

    Poissonzahl

    23.0 °C

    0.3 [-]

    Show Supplier Material materials with Poissonzahl of 0.3 [-]

    Streckgrenze Rp 0,2

    23.0 °C

    380 MPa

    Show Supplier Material materials with Streckgrenze Rp 0,2 of 380 MPa

    Zugfestigkeit

    23.0 °C

    470 MPa

    Show Supplier Material materials with Zugfestigkeit of 470 MPa

    Thermisch

    PropertyTemperatureValue

    Koeffizient der thermischen Ausdehnung

    23.0 °C

    1.7E-5 1/K

    Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 1/K

    Schmelzpunkt

    570 °C

    Show Supplier Material materials with Schmelzpunkt of 570 °C

    Spezifische Wärmekapazität

    23.0 °C

    850 J/(kg·K)

    Show Supplier Material materials with Spezifische Wärmekapazität of 850 J/(kg·K)

    Wärmeleitfähigkeit

    23.0 °C

    150 W/(m·K)

    Show Supplier Material materials with Wärmeleitfähigkeit of 150 W/(m·K)

    Technological properties

    Property
    Application areas

    Commercial and Military Aerospace: Outlet guide vanes, Hydraulic / Fuel blocks, Wheels, Fixed wing structure/ skins, Helicopter components - Commercial and Preformance Automotive: Pistons, Piston pins, Cylinder liners, Brake calipers, Connecting rods, Push rods, Valve train, Chassis components - Space, Defence and Optical Systems: Optical systems & sensors, Satellite structures, Astronomical telescopes

    Processing history

    Precision Extrusion