Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 1.64 g/cm³ Show Supplier Material materials with Dichte of 1.64 g/cm³ | ASTM D792 |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 234 MPa Show Supplier Material materials with Biegefestigkeit of 234 MPa | ASTM D790 |
Biegemodul | 23.0 °C | 14.48 GPa Show Supplier Material materials with Biegemodul of 14.48 GPa | ASTM D790 |
Dehnung | 23.0 °C | 1 - 2 % Show Supplier Material materials with Dehnung of 1 - 2 % | ASTM D638 |
Elastizitätsmodul | 23.0 °C | 15.86 GPa Show Supplier Material materials with Elastizitätsmodul of 15.86 GPa | ASTM D638 |
Impact strength, Izod notched, ASTM | 23.0 °C | 133 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 133 J/m | ASTM D256 |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 534 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 534 J/m | ASTM D4812 |
Zugfestigkeit | 23.0 °C | 165 MPa Show Supplier Material materials with Zugfestigkeit of 165 MPa | ASTM D638 |
Thermisch
Property | Value | Comment | |
---|---|---|---|
Heat deflection temperature, 1.80 MPa | 266 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 266 °C | ASTM D648 | |
Entflammbarkeit | HB ASTM D635, for 1.5mm |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Schrumpfung | 23.0 °C | 0.1 - 0.2 % Show Supplier Material materials with Schrumpfung of 0.1 - 0.2 % | ASTM D955, (1/8 in (3.2 mm)section) |
Technological properties
Property | ||
---|---|---|
Application areas | Chemical pump impeller, Valve core, Water heater connections, Water heater impeller, Chemical pump housing, Cooling water jacket. | |
Color | Natural, and custom colors | |
Fillers | 40% Glass Fiber | |
Processing methods | Injection Moulding. Injection Pressure 69 - 103 MPa, Melt Temperature 313 - 329 °C, Mould temperature 135 - 177 °C, Pre-drying 6 hrs @ 149 °C, Moisture Content 0.04% |