Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 2.17 g/cm³ Show Supplier Material materials with Dichte of 2.17 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Compressive yield strength | 23.0 °C | 147 MPa Show Supplier Material materials with Compressive yield strength of 147 MPa | |
Dauerfestigkeit | 23.0 °C | 86.2 MPa Show Supplier Material materials with Dauerfestigkeit of 86.2 MPa | 10⁷ cycles, R=-1, Kt=1 |
Dehnung | 23.0 °C | 4.7 % Show Supplier Material materials with Dehnung of 4.7 % | |
Elastizitätsmodul | 23.0 °C | 193 GPa Show Supplier Material materials with Elastizitätsmodul of 193 GPa | |
Poissonzahl | 23.0 °C | 0.15 [-] Show Supplier Material materials with Poissonzahl of 0.15 [-] | |
Scherfestigkeit | 23.0 °C | 181 MPa Show Supplier Material materials with Scherfestigkeit of 181 MPa | Pin Double Shear Strength |
Streckgrenze Rp 0,2 | 23.0 °C | 147.5 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 147.5 MPa | |
Zugfestigkeit | 23.0 °C | 196.5 MPa Show Supplier Material materials with Zugfestigkeit of 196.5 MPa |
Thermisch
Property | Temperature | Value |
---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.46E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.46E-5 1/K |
Spezifische Wärmekapazität | 23.0 °C | 1560 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 1560 J/(kg·K) |
Wärmeleitfähigkeit | 23.0 °C | 110 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 110 W/(m·K) |
Elektrisch
Property | Value |
---|---|
Specific Electrical conductivity | 48 % IACS Show Supplier Material materials with Specific Electrical conductivity of 48 % IACS |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Aluminium | Balance | ||
Beryllium | 56 - 68 % Show Supplier Material materials with Beryllium of 56 - 68 % | ||
Eisen | 0.45 % Show Supplier Material materials with Eisen of 0.45 % | max. | |
Germanium | 0.2 % Show Supplier Material materials with Germanium of 0.2 % | max. | |
Kobalt | 0.2 % Show Supplier Material materials with Kobalt of 0.2 % | max | |
Nickel | 2.4 - 3.5 % Show Supplier Material materials with Nickel of 2.4 - 3.5 % | ||
Silber | 0.2 % Show Supplier Material materials with Silber of 0.2 % | max. | |
Silizium | 0.2 % Show Supplier Material materials with Silizium of 0.2 % | max. |