Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 2.17 g/cm³ Show Supplier Material materials with Dichte of 2.17 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Compressive yield strength | 23.0 °C | 226.1 MPa Show Supplier Material materials with Compressive yield strength of 226.1 MPa | |
Dauerfestigkeit | 23.0 °C | 117.2 MPa Show Supplier Material materials with Dauerfestigkeit of 117.2 MPa | 10⁷ cycles, R=-1, Kt=1 |
Dehnung | 23.0 °C | 3 % Show Supplier Material materials with Dehnung of 3 % | |
Elastizitätsmodul | 23.0 °C | 193 GPa Show Supplier Material materials with Elastizitätsmodul of 193 GPa | |
Poissonzahl | 23.0 °C | 0.2 [-] Show Supplier Material materials with Poissonzahl of 0.2 [-] | |
Scherfestigkeit | 23.0 °C | 247.5 MPa Show Supplier Material materials with Scherfestigkeit of 247.5 MPa | Pin Double Shear Strength |
Streckgrenze Rp 0,2 | 23.0 °C | 213.7 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 213.7 MPa | |
Zugfestigkeit | 23.0 °C | 289.6 MPa Show Supplier Material materials with Zugfestigkeit of 289.6 MPa |
Thermisch
Property | Temperature | Value |
---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.42E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.42E-5 1/K |
Spezifische Wärmekapazität | 23.0 °C | 1250 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 1250 J/(kg·K) |
Wärmeleitfähigkeit | 23.0 °C | 105.5 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 105.5 W/(m·K) |
Elektrisch
Property | Value |
---|---|
Specific Electrical conductivity | 40 % IACS Show Supplier Material materials with Specific Electrical conductivity of 40 % IACS |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Aluminium | Balance | ||
Beryllium | 61.1 - 68.6 % Show Supplier Material materials with Beryllium of 61.1 - 68.6 % | ||
Eisen | 0.45 % Show Supplier Material materials with Eisen of 0.45 % | max. | |
Germanium | 0.55 - 0.95 % Show Supplier Material materials with Germanium of 0.55 - 0.95 % | ||
Kobalt | 0.65 - 1.35 % Show Supplier Material materials with Kobalt of 0.65 - 1.35 % | ||
Nickel | 0.2 % Show Supplier Material materials with Nickel of 0.2 % | max. | |
Silber | 2.65 - 3.35 % Show Supplier Material materials with Silber of 2.65 - 3.35 % | ||
Silizium | 0.2 % Show Supplier Material materials with Silizium of 0.2 % | max. |
Technological properties