Allgemein
Property | Value | Testing Standard | Comment |
---|---|---|---|
Dichte | 1.34 - 1.35 g/cm³ Show Supplier Material materials with Dichte of 1.34 - 1.35 g/cm³ | Depending on the thickness of the specimen | |
Moisture absorption | 1.1 % Show Supplier Material materials with Moisture absorption of 1.1 % | ASTM D348 |
Mechanisch
Property | Value | Comment |
---|---|---|
Biegefestigkeit | 60 - 75.8 MPa Show Supplier Material materials with Biegefestigkeit of 60 - 75.8 MPa | Minimum value for ISSC |
Biegemodul | 3.5 - 5.2 GPa Show Supplier Material materials with Biegemodul of 3.5 - 5.2 GPa | Minimum value for ISSC |
Druckfestigkeit | 137.9 MPa Show Supplier Material materials with Druckfestigkeit of 137.9 MPa | |
Härte, Rockwell M | 70 [-] Show Supplier Material materials with Härte, Rockwell M of 70 [-] | |
Kompressionsmodul | 4.1 GPa Show Supplier Material materials with Kompressionsmodul of 4.1 GPa | |
Zugfestigkeit | 37.9-51 | Depending on the thickness of the specimen |
Thermisch
Property | Value | Comment |
---|---|---|
Relative temperature index, mechanical strength | 165 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 165 °C | ¹ |
Technological properties
Property | ||
---|---|---|
Application areas | It is used as a bearing material or in other wear applications. | |
Fillers | Aramid Fiber | |
Other | 1.This temperature is a recommendation only, and based upon experience in various applications. The maximum operating temperature is dependent upon the application and should be investigated prior to use 2.The mechanical properties are converted from American unit system to International unit system. | |
Supplier Disclaimer | This data, while believed to be accurate and based on reliable analytical methods, is for informational purposes only. The terms and conditions of the agreement under which it is sold will govern any sales of this product. Data supplied above are "typical values"; not to be considered "specification values". To assure the material's performance is adequate for a specific application; customers should verify, independent of Norplex-Micarta, performance characteristics of interest. It is the responsibility of the users of this information to make sure that they have the latest version of this TDB, and are urged to check with Customer Service or, preferably our web site, www.norplex-micarta.com, to determine if the information is the most current available. |