Allgemein
Property | Value |
---|---|
Dichte | 2.34 g/cm³ Show Supplier Material materials with Dichte of 2.34 g/cm³ |
Mechanisch
Thermisch
Property | Temperature | Value | Testing Standard | Comment |
---|---|---|---|---|
Glasübergangstemperatur | 565 °C Show Supplier Material materials with Glasübergangstemperatur of 565 °C | ISO 7884-8 | ||
Glühtemperatur | 565.0 °C Show Supplier Material materials with Glühtemperatur of 565.0 °C | ISO 7884-4 | Viscosity 10¹³ dPa·s | |
Koeffizient der thermischen Ausdehnung | 4.9e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 4.9e-06 1/K | ISO 7991 | mean value for 20-300 °C | |
Softening temperature | 785.0 °C Show Supplier Material materials with Softening temperature of 785.0 °C | ISO 7884-3 | Viscosity 10⁷·⁶ dPa·s | |
Specific electrical resistance temperature | 215.0 °C Show Supplier Material materials with Specific electrical resistance temperature of 215.0 °C | For ρ=10⁸ Ω·cm | ||
Working temperature | 1160.0 °C Show Supplier Material materials with Working temperature of 1160.0 °C | ISO 7884-2 | Viscosity 10⁴ dPa·s | |
Wärmeleitfähigkeit | 90 °C | 1.2 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 1.2 W/(m·K) |
Elektrisch
Optisch
Property | Value | Testing Standard | Comment |
---|---|---|---|
Brechungsindex | 1.5 [-] Show Supplier Material materials with Brechungsindex of 1.5 [-] | at λ=587.6 nm | |
Stress optical coefficient | 3.4e-06 mm²/N Show Supplier Material materials with Stress optical coefficient of 3.4e-06 mm²/N | DIN 52314 |
Chemical properties
Property | Value | Comment |
---|---|---|
Aluminium | 5 % Show Supplier Material materials with Aluminium of 5 % | Al₂O₃ |
Bor | 10.5 % Show Supplier Material materials with Bor of 10.5 % | B₂O₃ |
Kalzium | 1.5 % Show Supplier Material materials with Kalzium of 1.5 % | CaO |
Natrium | 7 % Show Supplier Material materials with Natrium of 7 % | Na₂O |
Silizium | 75 % Show Supplier Material materials with Silizium of 75 % | SiO₂ |
Technological properties
Property | ||
---|---|---|
Application areas | Pharmaceutical packaging (Ampoules, Vials, Tablet bottles, Cartridges, Syringes). | |
Corrosion properties | Hydrolytic resistance Class HGB1 (ISO 719), Type I (Ph. Eur.), Type I (USP), Fullfield (JP) - Acid resistance Class S1 (DIN 12116) - Alkali resistance Class A2 (ISO695), ASTM E 438 Type I Class B |