Allgemein
Property | Value |
---|---|
Dichte | 2.67 g/cm³ Show Supplier Material materials with Dichte of 2.67 g/cm³ |
Mechanisch
Thermisch
Property | Temperature | Value | Testing Standard | Comment |
---|---|---|---|---|
Belastungstemperatur | 750 °C Show Supplier Material materials with Belastungstemperatur of 750 °C | ISO 7884-7 | Viscosity 10¹⁴·⁵ dPa·s | |
Glasübergangstemperatur | 790 °C Show Supplier Material materials with Glasübergangstemperatur of 790 °C | ISO 7884-8 | ||
Glühtemperatur | 795.0 °C Show Supplier Material materials with Glühtemperatur of 795.0 °C | ISO 7884-4 | Viscosity 10¹³ dPa·s | |
Koeffizient der thermischen Ausdehnung | 4.7e-06 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 4.7e-06 1/K | ISO 7991 | mean value for 20-300 °C | |
Softening temperature | 1005.0 °C Show Supplier Material materials with Softening temperature of 1005.0 °C | ISO 7884-3 | Viscosity 10⁷·⁶ dPa·s | |
Specific electrical resistance temperature | 630.0 °C Show Supplier Material materials with Specific electrical resistance temperature of 630.0 °C | For ρ=10⁸ Ω·cm | ||
Working temperature | 1305.0 °C Show Supplier Material materials with Working temperature of 1305.0 °C | ISO 7884-2 | Viscosity 10⁴ dPa·s | |
Wärmeleitfähigkeit | 90 °C | 1.1 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 1.1 W/(m·K) |
Elektrisch
Property | Temperature | Value | Frequency |
---|---|---|---|
Dielektrizitätskonstante | 6.6 [-] Show Supplier Material materials with Dielektrizitätskonstante of 6.6 [-] | 1MHz | |
Verlustfaktor | 0.0015 [-] Show Supplier Material materials with Verlustfaktor of 0.0015 [-] | 1MHz | |
spezifischer Widerstand | 250 °C | 1e+11 Ω·m Show Supplier Material materials with spezifischer Widerstand of 1e+11 Ω·m | |
350 °C | 1e+09 Ω·m Show Supplier Material materials with spezifischer Widerstand of 1e+09 Ω·m |
Optisch
Property | Value | Testing Standard | Comment |
---|---|---|---|
Brechungsindex | 1.5 [-] Show Supplier Material materials with Brechungsindex of 1.5 [-] | at λ=587.6 nm | |
Stress optical coefficient | 2.7e-06 mm²/N Show Supplier Material materials with Stress optical coefficient of 2.7e-06 mm²/N | DIN 52314 | |
UV transmission | 72 % Show Supplier Material materials with UV transmission of 72 % | max. | Thickness=1 mm | λ=330 nm |
Chemical properties
Property | ||
---|---|---|
Other | 0.01 % | max., Lead, Cadmium, Mercury and Hexavalent Chromium |
Technological properties
Property | ||
---|---|---|
Application areas | For high temperature applications in electrical engineering. For use in bulb and exhaust tube, for halogen lamps for automotive, houshold, general lighting and Exterior lighting | |
Corrosion properties | Hydrolytic resistance Class HGB1 (ISO 719) - Acid resistance Class S2 (DIN 12116) - Alkali resistance Class A2 (ISO695) |