Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 1.42 g/cm³ Show Supplier Material materials with Dichte of 1.42 g/cm³ | ASTM D792 |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 310 MPa Show Supplier Material materials with Biegefestigkeit of 310 MPa | ASTM D790 |
Biegemodul | 23.0 °C | 1.71 GPa Show Supplier Material materials with Biegemodul of 1.71 GPa | ASTM D790 |
Dehnung | 23.0 °C | 5.1 % Show Supplier Material materials with Dehnung of 5.1 % | ASTM D638 |
Impact strength, Izod notched, ASTM | 23.0 °C | 18 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 18 J/m | ASTM D256, 3.2mm |
Zugfestigkeit | 23.0 °C | 49 MPa Show Supplier Material materials with Zugfestigkeit of 49 MPa | ASTM D638 |
Thermisch
Property | Value | Comment | |
---|---|---|---|
Heat deflection temperature, 0.45 MPa | 320 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 320 °C | ASTM D648 | |
Entflammbarkeit | V2 UL94 |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
Surface resistivity | 23.0 °C | 1000 - 100000 Ω/sq Show Supplier Material materials with Surface resistivity of 1000 - 100000 Ω/sq | ASTM D257 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Schmelzmassenflussrate | 7.5 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 7.5 g/10min | ASTM D1238, 230°C/5kg | |
Schrumpfung | 23.0 °C | 0.15 - 0.2 % Show Supplier Material materials with Schrumpfung of 0.15 - 0.2 % | ASTM D1238, Mold Shrinkage |
Technological properties
Property | ||
---|---|---|
Application areas | ESD IC tray, ESD lens tray, Conductive tweenzers, ESD container, ESD electric & housing spare parts, Conductive communication equipment | |
Certifications | RoHS | |
Color | Black | |
Processing methods | Injection molding - Drying time: 4hrs, temperature: 120°C - Mold temperature:100-120°C - injection temperature: 120°C |