Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 1.11 g/cm³ Show Supplier Material materials with Dichte of 1.11 g/cm³ | ASTM D792 |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 63 MPa Show Supplier Material materials with Biegefestigkeit of 63 MPa | ASTM D790 |
Biegemodul | 23.0 °C | 1.44 GPa Show Supplier Material materials with Biegemodul of 1.44 GPa | ASTM D790 |
Dehnung | 23.0 °C | 37 % Show Supplier Material materials with Dehnung of 37 % | ASTM D638 |
Impact strength, Izod notched, ASTM | 23.0 °C | 13 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 13 J/m | ASTM D256 |
Zugfestigkeit | 23.0 °C | 34 MPa Show Supplier Material materials with Zugfestigkeit of 34 MPa | ASTM D638 |
Thermisch
Property | Value | Comment |
---|---|---|
Heat deflection temperature, 0.45 MPa | 73 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 73 °C | ASTM D648 |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
Surface resistivity | 23.0 °C | 1.00E+8 - 1.00E+9 Ω/sq Show Supplier Material materials with Surface resistivity of 1.00E+8 - 1.00E+9 Ω/sq | ASTM D257 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Schmelzmassenflussrate | 17.28 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 17.28 g/10min | ASTM D1238, 230°C/5kg | |
Schrumpfung | 23.0 °C | 0.94 % Show Supplier Material materials with Schrumpfung of 0.94 % | ASTM D1238, Mold Shrinkage |
Technological properties
Property | ||
---|---|---|
Certifications | RoHS | |
Processing methods | Injection molding - Drying time: 4hrs, temperature: 80°C - Injection temperature: 180-220°C |