Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 1.25 g/cm³ Show Supplier Material materials with Dichte of 1.25 g/cm³ | ASTM D792 |
Wasserabsorption | 23.0 °C | 0.38 % Show Supplier Material materials with Wasserabsorption of 0.38 % | ASTM D570, 24hr and 50%RH |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 160 MPa Show Supplier Material materials with Biegefestigkeit of 160 MPa | ASTM D790 |
Biegemodul | 23.0 °C | 4.89 GPa Show Supplier Material materials with Biegemodul of 4.89 GPa | ASTM D790 |
Dehnung | 23.0 °C | 10 % Show Supplier Material materials with Dehnung of 10 % | ASTM D638 |
Impact strength, Izod notched, ASTM | 23.0 °C | 5.1 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 5.1 J/m | ASTM D256 |
Zugfestigkeit | 23.0 °C | 105 MPa Show Supplier Material materials with Zugfestigkeit of 105 MPa | ASTM D638 |
Thermisch
Property | Value | Comment |
---|---|---|
Heat deflection temperature, 1.80 MPa | 140 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 140 °C | ASTM D648 |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
Surface resistivity | 23.0 °C | 10000 - 1000000 Ω/sq Show Supplier Material materials with Surface resistivity of 10000 - 1000000 Ω/sq | ASTM D257 |
Rheological Properties
Property | Value | Comment |
---|---|---|
Schmelzmassenflussrate | 10 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 10 g/10min | ASTM D2240, 180°C/5kg |
Technological properties
Property | ||
---|---|---|
Certifications | RoHS | |
Color | Black | |
Processing methods | Injection molding - Drying time: 4hrs, temperature: 140°C - mold temperature: 130-160°C - injection temperature: 250-290°C |