General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 2.68 g/cm³ Show Supplier Material materials with Densidad of 2.68 g/cm³ |
Medidas
Property | Value |
---|---|
Espesor | 0.2 - 6 mm Show Supplier Material materials with Espesor of 0.2 - 6 mm |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Brinell (HBW) | 23.0 °C | 63 [-] Show Supplier Material materials with Dureza Brinell (HBW) of 63 [-] |
Elongación A50 | 23.0 °C | 4 % Show Supplier Material materials with Elongación A50 of 4 % |
Límite elástico | 23.0 °C | 160 MPa Show Supplier Material materials with Límite elástico of 160 MPa |
Módulo de cizallamiento | 23.0 °C | 26.5 GPa Show Supplier Material materials with Módulo de cizallamiento of 26.5 GPa |
Módulo elástico | 23.0 °C | 70 GPa Show Supplier Material materials with Módulo elástico of 70 GPa |
Resistencia a la tracción | 23.0 °C | 210 - 260 MPa Show Supplier Material materials with Resistencia a la tracción of 210 - 260 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de dilatación térmica | 100.0 °C | 2.4E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 2.4E-5 1/K | 20-100°C |
Conductividad térmica | 23.0 °C | 138 W/(m·K) Show Supplier Material materials with Conductividad térmica of 138 W/(m·K) |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 23.0 °C | 4.9E-8 Ω·m Show Supplier Material materials with Resistividad eléctrica of 4.9E-8 Ω·m |
Chemical properties
Property | Value |
---|---|
Cobre | 0.1 % Show Supplier Material materials with Cobre of 0.1 % |
Cromo | 0.15 - 0.35 % Show Supplier Material materials with Cromo of 0.15 - 0.35 % |
Hierro | 0.4 % Show Supplier Material materials with Hierro of 0.4 % |
Magnesio | 2.2 - 2.8 % Show Supplier Material materials with Magnesio of 2.2 - 2.8 % |
Manganeso | 0.1 % Show Supplier Material materials with Manganeso of 0.1 % |
Otro | 0.15 % Show Supplier Material materials with Otro of 0.15 % |
Silicona | 0.25 % Show Supplier Material materials with Silicona of 0.25 % |
Zinc | 0.1 % Show Supplier Material materials with Zinc of 0.1 % |
Technological properties
Property | ||
---|---|---|
Anodizing | Excellent (anodizing quality) | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing quality; Electronic devices: Housing devices; Closures: Easy open; Food can: Body, Lids; Components: Heat shields, Access hatches, Spoilers, General trasportation | |
Corrosion properties | Excellent | |
Welding | Very Good | |
Workability | Good (in O temper) |