General
Property | Value | Comment |
---|---|---|
Carbon equivalent (CEV) | 0.23 [-] Show Supplier Material materials with Carbon equivalent (CEV) of 0.23 [-] | max. |
Medidas
Property | Value |
---|---|
Dimensions | *Pickled products with thicknesses up to 15 mm may be delivered after prior agreement: please contact us. Please feel free to check the figure on the right side of the material page for more details. |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 25 % Show Supplier Material materials with Elongación of 25 % | min. | for thickness < 3 mm | Transverse, A80 | |
26 % Show Supplier Material materials with Elongación of 26 % | min. | for thickness < 3 mm, A80 | ||
29 % Show Supplier Material materials with Elongación of 29 % | min. A5.65√So | for thickness 3-16 mm | Transverse | ||
30 % Show Supplier Material materials with Elongación of 30 % | min. A5.65√So | for thickness 3-16 mm | ||
Energía de impacto Charpy | -20 °C | 40 J Show Supplier Material materials with Energía de impacto Charpy of 40 J | min. | for thickness 6-16 mm |
Límite elástico | 280 - 350 MPa Show Supplier Material materials with Límite elástico of 280 - 350 MPa | for thickness < 16 mm | |
300 - 380 MPa Show Supplier Material materials with Límite elástico of 300 - 380 MPa | for thickness < 16 mm | Transverse | ||
Resistencia a la tracción | 370 - 450 MPa Show Supplier Material materials with Resistencia a la tracción of 370 - 450 MPa | for thickness < 16 mm | Transverse/Longitudinal |
Chemical properties
Property | Value | Comment |
---|---|---|
Aluminio | 0.015 % Show Supplier Material materials with Aluminio of 0.015 % | min. |
Azufre | 0.015 % Show Supplier Material materials with Azufre of 0.015 % | max. |
Carbono | 0.08 % Show Supplier Material materials with Carbono of 0.08 % | max. |
Fósforo | 0.02 % Show Supplier Material materials with Fósforo of 0.02 % | max. |
Manganeso | 0.8 % Show Supplier Material materials with Manganeso of 0.8 % | max. |
Niobio | 0.025 % Show Supplier Material materials with Niobio of 0.025 % | max. |
Silicona | 0.03 % Show Supplier Material materials with Silicona of 0.03 % | max. |
Titanio | 0.15 % Show Supplier Material materials with Titanio of 0.15 % | max. |
Vanadio | 0.2 % Show Supplier Material materials with Vanadio of 0.2 % | max. |
Technological properties
Property | ||
---|---|---|
Application areas | High strength Amstrong® steels are used in a wide range of applications in transport (earth movers, trailers, agricultural and railroad machinery etc), profiling (racks etc) and building (cranes, safety barriers, light poles etc). Significant weight reductions can be achieved by using Amstrong® steels, especially for cranes and heavy vehicle trailers, thus allowing a larger payload. | |
Chemical composition | The chemical properties given are based on cast analysis data. | |
Coating | Galvanisation: Class 1 Suitability for hot-dip zinc coating is defined as per the requirements of EN ISO 14713-2 Table 1 and NFA 35-503. | |
Other | Toughness guarantee at -40°C: on request |