General
Property | Value | Comment |
---|---|---|
Carbon equivalent (CEV) | 0.4 [-] Show Supplier Material materials with Carbon equivalent (CEV) of 0.4 [-] | max. |
Medidas
Property | Value |
---|---|
Dimensions | For thicknesses over 20 mm, please contact us. Please feel free to check the figure on the right side of the material page for more details. |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Drop-weight tear test | 10 °C | 100 % Show Supplier Material materials with Drop-weight tear test of 100 % | min. | for thickness 5-25 mm |
Elongación | 21 % Show Supplier Material materials with Elongación of 21 % | min. | for thickness 5-25 mm | Transverse | A50 | |
Energía de impacto Charpy | 0 °C | 40 J Show Supplier Material materials with Energía de impacto Charpy of 40 J | min. | for thickness 5-25 mm | Transverse |
Límite elástico | 320 - 525 MPa Show Supplier Material materials with Límite elástico of 320 - 525 MPa | for thickness 5-25 mm | Transverse | |
Resistencia a la tracción | 435 - 620 MPa Show Supplier Material materials with Resistencia a la tracción of 435 - 620 MPa | for thickness 5-25 mm | Transverse | |
Yield to strength ratio | 0.85 [-] Show Supplier Material materials with Yield to strength ratio of 0.85 [-] | for thickness 5-25 mm | Transverse |
Chemical properties
Property | Value | Comment |
---|---|---|
Aluminio | 0.015 - 0.06 % Show Supplier Material materials with Aluminio of 0.015 - 0.06 % | |
Azufre | 0.015 % Show Supplier Material materials with Azufre of 0.015 % | max. |
Carbono | 0.22 % Show Supplier Material materials with Carbono of 0.22 % | max. |
Cobre | 0.25 % Show Supplier Material materials with Cobre of 0.25 % | max. |
Cromo | 0.3 % Show Supplier Material materials with Cromo of 0.3 % | max. |
Fósforo | 0.025 % Show Supplier Material materials with Fósforo of 0.025 % | max. |
Manganeso | 1.4 % Show Supplier Material materials with Manganeso of 1.4 % | max. |
Molibdeno | 0.1 % Show Supplier Material materials with Molibdeno of 0.1 % | max. |
Niobio | 0.05 % Show Supplier Material materials with Niobio of 0.05 % | max. |
Nitrógeno | 0.012 % Show Supplier Material materials with Nitrógeno of 0.012 % | max. |
Níquel | 0.3 % Show Supplier Material materials with Níquel of 0.3 % | max. |
Silicona | 0.45 % Show Supplier Material materials with Silicona of 0.45 % | max. |
Titanio | 0.04 % Show Supplier Material materials with Titanio of 0.04 % | max. |
Vanadio | 0.05 % Show Supplier Material materials with Vanadio of 0.05 % | max. |
Technological properties
Property | ||
---|---|---|
Application areas | ArcelorMittal's steels for pipes are particularly suitable for manufacturing: Spiral SAW and straight ERW pipes made with this type of steel are a good alternative to UOE pipes (made from plate from quarto roll mills) or seamless pipes. These steels are used for the production of pipes for the transport of gaseous or liquid materials such as water or oil. | |
Chemical composition | Notes: 1.A ratio Al/N ≥ 2 shall be applied. 2. The sum of the percentages by mass of the three elements niobium, titanium and vanadium shall not exceed 0.15%. | |
Hydrogen induced cracking | HIC-resistant Since the dimensions available are constantly changing, please contact us for specific information. | |
Other | The mechanical properties of the pipes will depend on:
The evolution of the mechanical properties - and in particular of the difference in yield strength between the sheet and the pipe - is specific for each process. It is therefore very important to indicate both the forming and the welding process as well as the aforementioned sheet/pipe difference. An agreement between ArcelorMittal and the client on the coil mechanical properties to be guaranteed must be reached prior to delivery of the coils. The mechanical properties listed above are those of the pipes. The minimum elongation given above refers to a 610 mm diameter pipe with a wall thickness of 12.7 mm. | |
Welding | The chemical composition of this steel ensures that there is no risk of cold cracking and simply applying the normal welding rules is sufficient to achieve a good quality weld. For SAW welding, the choice of an SA1 AM FCE flux/wire combination for grades up to X46 AM FCE, and an SA2 AM FCE for higher grades, should produce a weld with a coefficient greater than 1 and a good degree of toughness at the centre of the weld. |