Medidas
Property | Value |
---|---|
Dimensions | Please feel free to check the figure on the right side of the material page for more details. |
Mecánica
Property | Value | Comment |
---|---|---|
Elongación | 32 % Show Supplier Material materials with Elongación of 32 % | min. | for thickness 0.3-2 mm | Transverse | A80 |
Límite elástico | 180 - 280 MPa Show Supplier Material materials with Límite elástico of 180 - 280 MPa | for thickness 0.3-2 mm | Transverse |
Resistencia a la tracción | 300 - 360 MPa Show Supplier Material materials with Resistencia a la tracción of 300 - 360 MPa | for thickness 0.3-2 mm | Transverse |
Chemical properties
Property | Value | Comment |
---|---|---|
Aluminio | 0.02 % Show Supplier Material materials with Aluminio of 0.02 % | min. |
Azufre | 0.025 % Show Supplier Material materials with Azufre of 0.025 % | max. |
Carbono | 0.08 % Show Supplier Material materials with Carbono of 0.08 % | max. |
Fósforo | 0.03 % Show Supplier Material materials with Fósforo of 0.03 % | max. |
Manganeso | 0.5 % Show Supplier Material materials with Manganeso of 0.5 % | max. |
Silicona | 0.03 % Show Supplier Material materials with Silicona of 0.03 % | max. |
Technological properties
Property | ||
---|---|---|
Application areas | This steel is used for the manufacture of casing panels for domestic appliances, heating equipment, furniture, shelving, drums and generally all applications where surface cleanliness is required. | |
Coating | Galvanisation: Class 1 | |
Surface condition | This cold rolled steel is available with surface types A or B as defined in the EN 10130 standard. | |
Welding | The weldability of this cold rolled grade using conventional processes is guaranteed. Nevertheless, it is recommended that the welding process should be specified when ordering. This grade is also suitable substrates for coatings such as phosphating, painting, electroplating and batch galvanisation. |