DILLIDUR 500

Want to keep this datasheet? Save it now in your required format

Description

DILLIDUR 500 is a wear resistant steel with a nominal hardness of 500 HBW in delivery condition ex works.

DILLIDUR 500 is preferentially used by the customers where very high resistance to wear is required together with good workability and especially good weldability.

In spite of their high tensile properties, DILLIDUR steels are not intended for safety relevant components. For this purpose high strength steels DILLIMAX are available.

Related Standards

Los datos sobre este material han sido proporcionados por Dillinger.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

Propiedades

General

PropertyValueComment

Carbon equivalent (CET)

0.39 [-]

Show Supplier Material materials with Carbon equivalent (CET) of 0.39 [-]

indicative values for thickness 10 mm

0.41 [-]

Show Supplier Material materials with Carbon equivalent (CET) of 0.41 [-]

indicative values for thickness 40 mm

0.44 [-]

Show Supplier Material materials with Carbon equivalent (CET) of 0.44 [-]

indicative values for thickness 80 mm

Carbon equivalent (CEV)

0.53 [-]

Show Supplier Material materials with Carbon equivalent (CEV) of 0.53 [-]

indicative values for thickness 10 mm

0.57 [-]

Show Supplier Material materials with Carbon equivalent (CEV) of 0.57 [-]

indicative values for thickness 40 mm

0.67 [-]

Show Supplier Material materials with Carbon equivalent (CEV) of 0.67 [-]

indicative values for thickness 80 mm

Carbon equivalent note

CEV = C + Mn/6 + (Cr+Mo+V)/5 + (Cu+Ni)/15 and CET = C + (Mn+Mo)/10 + (Cr+Cu)/20 + Ni/40

Mecánica

PropertyTemperatureValueComment

Charpy impact energy, V-notch

-20 °C

25 J

Show Supplier Material materials with Charpy impact energy, V-notch of 25 J

indicative values for 20 mm plate thickness

Dureza Brinell

450 [-]

Show Supplier Material materials with Dureza Brinell of 450 [-]

HBW for plate thicknesses > 30 mm (1.2 in.) The approximately converted values in brackets are for information only.

470 [-]

Show Supplier Material materials with Dureza Brinell of 470 [-]

HBW for plate thicknesses ≤ 30 mm (1.2 in.) The approximately converted values in brackets are for information only.

Elongación

9 %

Show Supplier Material materials with Elongación of 9 %

indicative values for 20 mm plate thickness | transverse specimens at room temperature, A5

Límite elástico

1100 MPa

Show Supplier Material materials with Límite elástico of 1100 MPa

indicative values for 20 mm plate thickness | transverse specimens at room temperature

Resistencia a la tracción

1600 MPa

Show Supplier Material materials with Resistencia a la tracción of 1600 MPa

indicative values for 20 mm plate thickness | transverse specimens at room temperature

Chemical properties

PropertyValueComment

Azufre

0.01 %

Show Supplier Material materials with Azufre of 0.01 %

max.

Boro

0.005 %

Show Supplier Material materials with Boro of 0.005 %

max.

Carbono

0.3 %

Show Supplier Material materials with Carbono of 0.3 %

max.

Cobre

0.3 %

Show Supplier Material materials with Cobre of 0.3 %

max.

Cromo

1.5 %

Show Supplier Material materials with Cromo of 1.5 %

max.

Fósforo

0.025 %

Show Supplier Material materials with Fósforo of 0.025 %

max.

Hierro

Balance

Manganeso

1.6 %

Show Supplier Material materials with Manganeso of 1.6 %

max.

Molibdeno

0.5 %

Show Supplier Material materials with Molibdeno of 0.5 %

max.

Niobio

0.05 %

Show Supplier Material materials with Niobio of 0.05 %

max.

Níquel

1 %

Show Supplier Material materials with Níquel of 1 %

max.

Silicona

0.7 %

Show Supplier Material materials with Silicona of 0.7 %

max.

Vanadio

0.08 %

Show Supplier Material materials with Vanadio of 0.08 %

max.

Technological properties

Property
Application areas

Examples of application: earth moving and loading machines, dredgers, skip cars, conveying plants, trucks, cutting edges, knives and breakers, waste elimination and recycling plants.

Chemical composition

Depending on thickness, the following alloying elements may be used singly or in combination: Mo, Ni, Cu, Cr, V, Nb and B.

Cold Forming

DILLIDUR 500 can be cold formed by bending in spite of its high hardness and strength. It should be paid attention to the fact that with increasing yield strength, the required forces for the forming operation also increase, even if the plate thickness remains unchanged. The spring-back also increases. Grinding of the flame cut or sheared edges in the bending area is recommended to avoid crack initiation. In order to avoid the risk of cracking from the edges, flame cut or sheared edges should be ground in the area that is to be cold formed. It is also advisable to round the plate edge slightly on the outside of the bend coming under tension stress during bending.

During the processing, the necessary safety measures have to be taken, so that nobody will be exposed to a danger by a possible fracture of the work piece during the forming process.

The following geometries can usually be achieved by cold forming without the formation of surface defects (where t is the plate thickness):


Position of bending line to rolling directionMinimum bending radiusMinimum die width
Transverse direction7 t16 t
Longitudinal direction9 t20 t

Delivery condtion

Controlled water quenched.

Unless otherwise agreed, the general technical requirements in accordance with EN 10021 are applicable.

Flame cutting and welding

For flame cutting, the following minimum temperatures should be observed: 60 °C (140 °F) for plate thicknesses up to 26 mm, 120 °C (248 °F) for plate thicknesses from 26 up to 70 mm and 150 °C (302 °F) for thicker plates.

For manual arc welding, basic coated rods with very low residual moisture should be used (and dried if necessary according to the manufacturer’s instructions).

Additionally the following recommendations are to be considered:

  • For more information about preheating of DILLIDUR 500, please refer to our technical information “THE CONCEPT TO COMBAT WEAR AND TEAR – DILLIDUR”. Preheating above 200 °C (390 F) must however be avoided, because it could cause a decrease of the hardness (see diagram).
  • Weld metals with low yield strength are preferred for tack, root and filler passes. If welds are exposed to wear, only the final passes should be welded with consumables producing a hardness matching the parent plate.

  • General note

    If special requirements, which are not covered in this material data sheet, are to be met by the steel due to its intended use or processing, these requirements are to be agreed before placing the order.

    The information in this data sheet is a product description. This data sheet is updated at irregular intervals. The current version is relevant. For more information about application and processing of DILLIDUR 500, please refer to our technical information “THE CONCEPT TO COMBAT WEAR AND TEAR – DILLIDUR”. The current version is available from the mill or as download at www.dillinger.de.

    Heat Treatment

    The diagram above in the picture part of the datasheet shows the general changes in hardness or strength values in accordance with the heat treatment temperature.

    Hot forming

    Since DILLIDUR 500 obtains its hardness by accelerated cooling from the austenitizing temperature, hot forming without major hardness loss is only possible if a renewed quenching treatment is carried out after forming. However, the hardness achieved by means of such a treatment may differ from that measured in the delivery condition. This is due to the fact that the cooling conditions at the fabricator’s works are generally less adequate than those available during plate production.

    The steel can be heated to about 200 °C (390 °F) without any substantial drop in hardness.

    Machining

    DILLIDUR 500 can be machined with HSS-drills and especially with HSS-Co-alloyed drills with a satisfactory service life if the drill advance and cutting speed are correspondingly accommodated.

    Other

    DILLIDUR 500 can be delivered in thicknesses from 8 mm (1/3 in.) to 100 mm (4 in.), according to the dimensional program. Other dimensions may be possible on request.


    Identification of plates Unless otherwise agreed the marking is carried out via steel stamps with at least the following information:

  • steel grade (DILLIDUR 500)
  • heat number
  • number of mother plate and individual plate
  • the manufacturer’s symbol
  • inspector’s sign

  • Processing history

    The steel is fully killed and fine grain treated.

    Processing methods

    The entire processing and application techniques are of fundamental importance to the reliability of the products made from this steel. The user should ensure that his design, construction and processing methods are aligned with the material, correspond to the state of the art that the fabricator has to comply with and are suitable for the intended use. The customer is responsible for the selection of the material. The recommendations in accordance with EN 1011-2 (Welding) and CEN/TR 10347 (Forming) as well as recommendations regarding job safety in accordance with national rules should be observed while considering the higher strength and hardenability.

    Surface condition

    Surface quality: Unless otherwise agreed, the provisions in accordance with EN 10163-2, class A2 are applicable.

    Testings

    Brinell surface hardness tested once per heat and 40 t.

    Tolerances

    Unless otherwise agreed, the tolerances are in accordance with EN 10029, with class A for thickness.