General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 8.4 g/cm³ Show Supplier Material materials with Densidad of 8.4 g/cm³ |
Medidas
Property | Value |
---|---|
Dimensions | Available size round products (mm): 1-20 |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Brinell | 23.0 °C | 103 - 166 [-] Show Supplier Material materials with Dureza Brinell of 103 - 166 [-] |
Dureza Rockwell C | 23.0 °C | 0 - 5 [-] Show Supplier Material materials with Dureza Rockwell C of 0 - 5 [-] |
Dureza Vickers | 23.0 °C | 110 - 170 [-] Show Supplier Material materials with Dureza Vickers of 110 - 170 [-] |
Elongación | 23.0 °C | 3 % Show Supplier Material materials with Elongación of 3 % |
Límite elástico | 23.0 °C | 250 - 400 MPa Show Supplier Material materials with Límite elástico of 250 - 400 MPa |
Módulo elástico | 23.0 °C | 100 GPa Show Supplier Material materials with Módulo elástico of 100 GPa |
Resistencia a la tracción | 23.0 °C | 450 - 600 MPa Show Supplier Material materials with Resistencia a la tracción of 450 - 600 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 2.1E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 2.1E-5 1/K | for 20-200°C |
Conductividad térmica | 23.0 °C | 113 W/(m·K) Show Supplier Material materials with Conductividad térmica of 113 W/(m·K) | for 20-200°C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Conductividad eléctrica | 23.0 °C | 1.50E+7 S/m Show Supplier Material materials with Conductividad eléctrica of 1.50E+7 S/m |
Technological properties
Property | ||
---|---|---|
Application areas | Summary of typical applications: Machined parts for optical and electronic industry, RoHS compliant | |
Corrosion properties | Corrosion resistance rating: 3 out of 5 | |
General machinability | Machinability: 70 % | |
Processing history | Condition: H14 |