General
Property | Value | Testing Standard |
---|---|---|
Densidad | 1.05 - 1.11 g/cm³ Show Supplier Material materials with Densidad of 1.05 - 1.11 g/cm³ | ASTM D792 |
Mecánica
Property | Temperature | Value | Testing Standard | Comment |
---|---|---|---|---|
Dureza Shore A | 27 - 33 [-] Show Supplier Material materials with Dureza Shore A of 27 - 33 [-] | ASTM D2240 | ||
Elongación | 587.1 % Show Supplier Material materials with Elongación of 587.1 % | ASTM D412 | 500 mm/min | |
Módulo a elongación del 300 % | 0.00085 GPa Show Supplier Material materials with Módulo a elongación del 300 % of 0.00085 GPa | ASTM D412 | 500 mm/min | |
Módulo al 100 % de elongación | 0.00049 GPa Show Supplier Material materials with Módulo al 100 % de elongación of 0.00049 GPa | ASTM D412 | 500 mm/min | |
Resistencia a desgarros | 7.5 kN/m Show Supplier Material materials with Resistencia a desgarros of 7.5 kN/m | ASTM D624 Die C | 500 mm/min | |
Resistencia a la tracción | 1.4 MPa Show Supplier Material materials with Resistencia a la tracción of 1.4 MPa | ASTM D412 | 500 mm/min | |
Set de compresión | 23 °C | 11.3 [-] Show Supplier Material materials with Set de compresión of 11.3 [-] | ASTM D395 B | |
70 °C | 85.8 [-] Show Supplier Material materials with Set de compresión of 85.8 [-] | ASTM D395 B |
Rheological Properties
Property | Value | Testing Standard | Comment |
---|---|---|---|
Contracción | 1.1 - 1.7 % Show Supplier Material materials with Contracción of 1.1 - 1.7 % | ASTM D955 | Transverse |
1.9 - 2.5 % Show Supplier Material materials with Contracción of 1.9 - 2.5 % | ASTM D955 | ||
Velocidad de flujo de la masa derretida | 40.8 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 40.8 g/10min | ASTM D1238 | 190°C/2.16kg |
Technological properties
Property | ||
---|---|---|
Application areas | Tool grip, bicycle grip | |
Certifications | REACH SVHC free, RoHS 2.0, GS AfPS GS 2019:01 PAK, EN 71-3 | |
Color | Black | |
Fillers | Calcium Carbonate | |
Other | Overmolding capabilities: PP |