General
Property | Value | Testing Standard |
---|---|---|
Densidad | 0.98 - 1.04 g/cm³ Show Supplier Material materials with Densidad of 0.98 - 1.04 g/cm³ | ASTM D792 |
Mecánica
Property | Value | Testing Standard | Comment |
---|---|---|---|
Dureza Shore A | 82 - 88 [-] Show Supplier Material materials with Dureza Shore A of 82 - 88 [-] | ASTM D2240 | |
Elongación | 292 % Show Supplier Material materials with Elongación of 292 % | ASTM D412 | 500 mm/min |
Módulo al 100 % de elongación | 0.00426 GPa Show Supplier Material materials with Módulo al 100 % de elongación of 0.00426 GPa | ASTM D412 | 500 mm/min |
Resistencia a desgarros | 33.9 kN/m Show Supplier Material materials with Resistencia a desgarros of 33.9 kN/m | ASTM D624 Die C | 500 mm/min |
Resistencia a la tracción | 4.9 MPa Show Supplier Material materials with Resistencia a la tracción of 4.9 MPa | ASTM D412 | 500 mm/min |
Rheological Properties
Property | Value | Testing Standard | Comment |
---|---|---|---|
Contracción | 0.8 - 1.4 % Show Supplier Material materials with Contracción of 0.8 - 1.4 % | ASTM D955 | Transverse |
1.2 - 1.8 % Show Supplier Material materials with Contracción of 1.2 - 1.8 % | ASTM D955 | ||
Velocidad de flujo de la masa derretida | 48.9 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 48.9 g/10min | ASTM D1238 | 190°C/2.16kg |
Technological properties
Property | ||
---|---|---|
Application areas | Tool grips, bushes | |
Certifications | REACH SVHC free, RoHS 2.0, GS AfPS GS 2019:01 PAK, EN 71-3 | |
Color | Black | |
Fillers | Calcium Carbonate | |
Other | Overmolding capabilities: PP |