General
Property | Value | Testing Standard |
---|---|---|
Densidad | 0.83 - 0.89 g/cm³ Show Supplier Material materials with Densidad of 0.83 - 0.89 g/cm³ | ASTM D792 |
Mecánica
Property | Value | Testing Standard | Comment |
---|---|---|---|
Elongación | 1288.7 % Show Supplier Material materials with Elongación of 1288.7 % | ASTM D412 | 500 mm/min |
Módulo a elongación del 300 % | 0.00012 GPa Show Supplier Material materials with Módulo a elongación del 300 % of 0.00012 GPa | ASTM D412 | 500 mm/min |
Módulo al 100 % de elongación | 8e-05 GPa Show Supplier Material materials with Módulo al 100 % de elongación of 8e-05 GPa | ASTM D412 | 500 mm/min |
Resistencia a desgarros | 5.0 kN/m Show Supplier Material materials with Resistencia a desgarros of 5.0 kN/m | ASTM D624 Die C | 500 mm/min |
Resistencia a la tracción | 1.3 MPa Show Supplier Material materials with Resistencia a la tracción of 1.3 MPa | ASTM D412 | 500 mm/min |
Rheological Properties
Property | Value | Testing Standard | Comment |
---|---|---|---|
Contracción | 0.6 - 1.2 % Show Supplier Material materials with Contracción of 0.6 - 1.2 % | ASTM D955 | Transverse |
1.5 - 2.1 % Show Supplier Material materials with Contracción of 1.5 - 2.1 % | ASTM D955 | ||
Velocidad de flujo de la masa derretida | 63.5 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 63.5 g/10min | ASTM D1238 | 130°C/2.16kg |
Technological properties
Property | ||
---|---|---|
Application areas | Gel pad, insole and many more… | |
Certifications | REACH SVHC free, RoHS 2.0, GS AfPS GS 2019:01 PAK, EN 71-3, Meets FDA requirements | |
Color | Transparent | |
Processing methods |