General
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of friction | 0.35 - 0.44 [-] Show Supplier Material materials with Coefficient of friction of 0.35 - 0.44 [-] | ||
Coefficient of friction, kinetic | 0.44 [-] Show Supplier Material materials with Coefficient of friction, kinetic of 0.44 [-] | ASTM D 3702 Modified: Manual | |
Coefficient of friction, static | 0.35 [-] Show Supplier Material materials with Coefficient of friction, static of 0.35 [-] | ASTM D 3702 Modified: Manual | |
Densidad | 23.0 °C | 1.7 g/cm³ Show Supplier Material materials with Densidad of 1.7 g/cm³ | ISO 1183 |
Moisture absorption | 23.0 °C | 0.01 % Show Supplier Material materials with Moisture absorption of 0.01 % | ISO 62 | (23°C / 50% RH) |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 1.3 % Show Supplier Material materials with Elongación of 1.3 % | ISO 527 | break, 5 mm/min |
Impact strength, Izod notched, ASTM | 23.0 °C | 60 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 60 J/m | ASTM D 256 | notched, 23°C |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 416 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 416 J/m | ASTM D 4812 | 23°C |
Instrumented Impact, Total Energy | 23.0 °C | 11 J Show Supplier Material materials with Instrumented Impact, Total Energy of 11 J | ASTM D 3763 | 23°C |
Instrumented Impact, at Peak | 23.0 °C | 3 J Show Supplier Material materials with Instrumented Impact, at Peak of 3 J | ASTM D 3763 | 23°C |
Módulo de flexión | 23.0 °C | 11.1 GPa Show Supplier Material materials with Módulo de flexión of 11.1 GPa | ISO 178 | 2 mm/min |
Módulo elástico | 23.0 °C | 12 GPa Show Supplier Material materials with Módulo elástico of 12 GPa | ISO 527 | 1 mm/min |
Resistencia a la flexión | 23.0 °C | 180 MPa Show Supplier Material materials with Resistencia a la flexión of 180 MPa | ISO 178 |
Resistencia a la tracción | 23.0 °C | 121 MPa Show Supplier Material materials with Resistencia a la tracción of 121 MPa | ISO 527 | break, 5 mm/min |
Resistencia al choque, ensayo Izod entallado | 23.0 °C | 5 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Izod entallado of 5 kJ/m² | ISO 180/1A | notched 80*10*4, 23°C |
Resistencia al choque, ensayo Izod no entallado | 23.0 °C | 24 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Izod no entallado of 24 kJ/m² | ISO 180/1U | 80*10*4, 23°C |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 2.4E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 2.4E-5 1/K | ISO 11359-2 | -40°C to 40°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 5E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica transversal of 5E-5 1/K | ISO 11359-2 | -40°C to 40°C | ||
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | IEC 60695-2-12 | 0.75 mm | |||
Glow Wire Ignition Temperature | 800 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 800 °C | IEC 60695-2-13 | 0.75 mm | |||
Heat deflection temperature, 0.45 MPa | 278 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 278 °C | ISO 75/Bf | Flatw 80*10*4 sp=64mm | |||
Heat deflection temperature, 1.80 MPa | 257 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 257 °C | ISO 75/Af | Flatw 80*10*4 sp=64mm | |||
Relative temperature index, electrical | 105 °C Show Supplier Material materials with Relative temperature index, electrical of 105 °C | UL 746B | |||
Relative temperature index, mechanical impact | 105 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 105 °C | UL 746B | |||
Relative temperature index, mechanical strength | 105 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 105 °C | UL 746B | |||
Temperatura de flexión bajo carga | 257 - 278 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 257 - 278 °C | ||||
Inflamabilidad | UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=101283823- - <br> UL Recognized, 94V-0 Flame Class Rating: 1.5mm UL 94 <br> UL Yellow Card Link 2: https://iq.ul.com/ul/cert.aspx?ULID=101282823- - <br> UL Yellow Card Link 3: https://iq.ul.com/ul/cert.aspx?ULID=101344460- - |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
High Amp Arc Ignition | 23.0 °C | 0.75 mm Show Supplier Material materials with High Amp Arc Ignition of 0.75 mm | ≥, UL 746A | PLC 2 |
High Volt Arc Track Rate | 23.0 °C | 4 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 4 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 1.5 mm Show Supplier Material materials with Hot-Wire Ignition of 1.5 mm | ≥, UL 746A | PLC 0 |
Índice de seguimiento comparativo | 23.0 °C | 4 V Show Supplier Material materials with Índice de seguimiento comparativo of 4 V | UL 746A | (UL) {PLC} |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Document Handling | |
Availability | Americas | |
Processing methods | Drying Temperature: 120 to 150.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |