General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.07 % Show Supplier Material materials with Absorción de agua of 0.07 % | ASTM D 570 | (23°C/24hrs) |
Densidad relativa | 23.0 °C | 1.16 [-] Show Supplier Material materials with Densidad relativa of 1.16 [-] | ASTM D 792 |
Índice límite de óxigeno | 23.0 °C | 33.9 % Show Supplier Material materials with Índice límite de óxigeno of 33.9 % |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 5 % Show Supplier Material materials with Elongación of 5 % | ASTM D 638 | brk, Type I, 5 mm/min |
Módulo de flexión | 23.0 °C | 4 GPa Show Supplier Material materials with Módulo de flexión of 4 GPa | ASTM D 790 | 1.3 mm/min, 50 mm span |
Resistencia a la flexión | 23.0 °C | 119 MPa Show Supplier Material materials with Resistencia a la flexión of 119 MPa | ASTM D 790 | brk, 1.3 mm/min, 50 mm span |
Resistencia a la tracción | 23.0 °C | 74 MPa Show Supplier Material materials with Resistencia a la tracción of 74 MPa | ASTM D 638 | brk, Type I, 5 mm/min |
Resistencia al choque, ensayo Izod entallado | 23.0 °C | 96 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Izod entallado of 96 kJ/m² | ASTM D 256 | notched, 23°C |
Aplicaciones térmicas
Property | Value | Comment | |
---|---|---|---|
Heat deflection temperature, 1.80 MPa | 131 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 131 °C | ASTM D 648 | 6.4 mm, unannealed | |
Relative temperature index, electrical | 110 °C Show Supplier Material materials with Relative temperature index, electrical of 110 °C | UL 746B | |
Relative temperature index, mechanical impact | 105 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 105 °C | UL 746B | |
Relative temperature index, mechanical strength | 110 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 110 °C | UL 746B | |
Temperatura de flexión bajo carga | 131 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 131 °C | ||
Temperatura de reblandecimiento Vicat | 147 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 147 °C | ASTM D 1525 | Rate B/50 | |
Inflamabilidad | UL Recognized, 94V-1 Flame Class Rating: ≥1.5mm UL 94 <br> UV-light, water exposure/immersion: F1- UL 746C <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=221214- - <br> UL Yellow Card Link 2: https://iq.ul.com/ul/cert.aspx?ULID=100072184- - |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Constante dieléctrica, 1 MHz | 23.0 °C | 3 [-] Show Supplier Material materials with Constante dieléctrica, 1 MHz of 3 [-] | ASTM D 150 |
Dielectric constant, 60Hz | 23.0 °C | 3 [-] Show Supplier Material materials with Dielectric constant, 60Hz of 3 [-] | ASTM D 150 | 50/60 Hz |
Dissipation factor, 1MHz | 23.0 °C | 1.6E-3 [-] Show Supplier Material materials with Dissipation factor, 1MHz of 1.6E-3 [-] | ASTM D 150 | |
Dissipation factor, 50Hz | 23.0 °C | 1.7E-3 [-] Show Supplier Material materials with Dissipation factor, 50Hz of 1.7E-3 [-] | ASTM D 150 | 50/60 Hz |
High Amp Arc Ignition | 23.0 °C | 1.5 mm Show Supplier Material materials with High Amp Arc Ignition of 1.5 mm | ≥, UL 746A | PLC 2 |
High Volt Arc Track Rate | 23.0 °C | 4 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 4 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 1.5 mm Show Supplier Material materials with Hot-Wire Ignition of 1.5 mm | ≥, UL 746A | PLC 1 |
Volume resistivity | 23.0 °C | 1.00E+15 Ω·cm Show Supplier Material materials with Volume resistivity of 1.00E+15 Ω·cm | ASTM D 257 |
Índice de seguimiento comparativo | 23.0 °C | 2 V Show Supplier Material materials with Índice de seguimiento comparativo of 2 V | UL 746A | (UL) {PLC} |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.3 % Show Supplier Material materials with Contracción of 0.3 % | SABIC method | on tensile bar |
Technological properties
Property | ||
---|---|---|
Application areas | Circuit Protection, Building Accessory, Auto Electrical, Battery Pack, Audio, Auto Aftermarket, Aerospace, Coffee Maker/Espresso Machine, Cladding/Roof, Document Handling, Displays, Dishwasher, Enclosures, Enclosure/Housing/Cover, Energy Management, Electronic Components, Humidity Control, Individual Equiptment, Eyeglasses, Freezer, Fixture Bath/Shower, Engine Component, EV/HEV Battery, Wiring Devices, Wireless Communications, Personal Computing, Monitoring and Imaging, Meter Gas, Medical Device, Respiratory, Plumbing, Photovoltaic Components, Power Manangement, Pump | |
Availability | Europe,Asia,Americas | |
Processing methods | Shot to Cylinder Size: 30 to 70.0% | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |