General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad relativa | 23.0 °C | 1.11 [-] Show Supplier Material materials with Densidad relativa of 1.11 [-] | ASTM D 792 | |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 17 % Show Supplier Material materials with Elongación of 17 % | ASTM D 638 | brk, Type I, 50 mm/min |
Impact strength, Izod notched, ASTM | 23.0 °C | 96 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 96 J/m | ASTM D 256 | notched, -30°C |
Instrumented Impact, at Peak | 23.0 °C | 39 J Show Supplier Material materials with Instrumented Impact, at Peak of 39 J | ASTM D 3763 | 23°C |
Módulo de flexión | 23.0 °C | 2.5 GPa Show Supplier Material materials with Módulo de flexión of 2.5 GPa | ASTM D 790 | 2.6 mm/min, 100 mm span |
Resistencia a la flexión | 23.0 °C | 99 MPa Show Supplier Material materials with Resistencia a la flexión of 99 MPa | ASTM D 790 | yld, 2.6 mm/min, 100 mm span |
Resistencia a la tracción | 23.0 °C | 66 MPa Show Supplier Material materials with Resistencia a la tracción of 66 MPa | ASTM D 638 | yld, Type I, 50 mm/min |
Resistencia al choque, ensayo Izod entallado | 23.0 °C | 186 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Izod entallado of 186 kJ/m² | ASTM D 256 | notched, 23°C |
Aplicaciones térmicas
Property | Value | Comment | |
---|---|---|---|
Heat deflection temperature, 0.45 MPa | 109 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 109 °C | ASTM D 648 | 6.4 mm, unannealed | |
Heat deflection temperature, 1.80 MPa | 99 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 99 °C | ASTM D 648 | 6.4 mm, unannealed | |
Relative temperature index, electrical | 95 °C Show Supplier Material materials with Relative temperature index, electrical of 95 °C | UL 746B | |
Relative temperature index, mechanical impact | 80 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 80 °C | UL 746B | |
Relative temperature index, mechanical strength | 95 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 95 °C | UL 746B | |
Temperatura de flexión bajo carga | 99 - 109 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 99 - 109 °C | ||
Temperatura de reblandecimiento Vicat | 128 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 128 °C | ASTM D 1525 | Rate B/50 | |
Inflamabilidad | UL Recognized, 94HB Flame Class Rating: ≥0.4mm UL 94 <br> Radiant Panel Listing: TRUE- UL Tested <br> UL Recognized, 94V-0 Flame Class Rating: ≥1.5mm UL 94 <br> UL Recognized, 94-5VA Flame Class Rating: ≥3mm UL 94 <br> UV-light, water exposure/immersion: F1- UL 746C <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=221178- - |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Constante dieléctrica, 1 MHz | 23.0 °C | 2.55 [-] Show Supplier Material materials with Constante dieléctrica, 1 MHz of 2.55 [-] | ASTM D 150 |
Dielectric constant, 60Hz | 23.0 °C | 2.69 [-] Show Supplier Material materials with Dielectric constant, 60Hz of 2.69 [-] | ASTM D 150 | 50/60 Hz |
Dissipation factor, 1MHz | 23.0 °C | 7E-3 [-] Show Supplier Material materials with Dissipation factor, 1MHz of 7E-3 [-] | ASTM D 150 |
Dissipation factor, 50Hz | 23.0 °C | 0.01 [-] Show Supplier Material materials with Dissipation factor, 50Hz of 0.01 [-] | ASTM D 150 | 50/60 Hz |
High Amp Arc Ignition | 23.0 °C | 1.5 mm Show Supplier Material materials with High Amp Arc Ignition of 1.5 mm | ≥, UL 746A | PLC 0 |
High Volt Arc Track Rate | 23.0 °C | 4 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 4 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 6 mm Show Supplier Material materials with Hot-Wire Ignition of 6 mm | ≥, UL 746A | PLC 0 |
Rigidez dieléctrica | 23.0 °C | 16.2 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 16.2 kV/mm | ASTM D 149 | in oil, 3.2 mm |
Sheet resistivity, ROA | 23.0 °C | 1.00E+14 Ω Show Supplier Material materials with Sheet resistivity, ROA of 1.00E+14 Ω | >, ASTM D 257 |
Volume resistivity | 23.0 °C | 2.80E+16 Ω·cm Show Supplier Material materials with Volume resistivity of 2.80E+16 Ω·cm | ASTM D 257 |
Índice de seguimiento comparativo | 23.0 °C | 1 V Show Supplier Material materials with Índice de seguimiento comparativo of 1 V | UL 746A | (UL) {PLC} |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | EV/HEV Battery, Food Processor, Enclosures, Electronic Components, Circuit Protection, Data Management, Data Transfer, Document Handling, Meter Gas, Respiratory, Security/Detection, Small Appliance, Power Manangement, Wiring Devices, Wireless Communications | |
Availability | Americas | |
Processing methods | Maximum Moisture Content: 0.02% | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |