General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad relativa | 23.0 °C | 1.25 [-] Show Supplier Material materials with Densidad relativa of 1.25 [-] | ASTM D 792 | |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 3.7 % Show Supplier Material materials with Elongación of 3.7 % | ISO 527 | yield |
Impact strength, Izod notched, ASTM | 23.0 °C | 131 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 131 J/m | ASTM D 256 | notched, 23°C |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 2230 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 2230 J/m | ASTM D 4812 | 23°C |
Instrumented Impact, Total Energy | 23.0 °C | 443 J Show Supplier Material materials with Instrumented Impact, Total Energy of 443 J | ASTM D 3763 | 23°C |
Módulo de flexión | 23.0 °C | 3.8 GPa Show Supplier Material materials with Módulo de flexión of 3.8 GPa | ISO 178 |
Módulo elástico | 23.0 °C | 4 GPa Show Supplier Material materials with Módulo elástico of 4 GPa | ISO 527 | 1 mm/min |
Resistencia a la flexión | 23.0 °C | 117 MPa Show Supplier Material materials with Resistencia a la flexión of 117 MPa | ISO 178 |
Resistencia a la tracción | 23.0 °C | 57 MPa Show Supplier Material materials with Resistencia a la tracción of 57 MPa | ISO 527 | break |
Resistencia al choque, ensayo Charpy entallado | 23.0 °C | 10 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 10 kJ/m² | ISO 179/2C | 23°C |
Resistencia al choque, ensayo Izod entallado | 23.0 °C | 9 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Izod entallado of 9 kJ/m² | ISO 180/1A | notched 80*10*4, 23°C |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 7.06E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 7.06E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 7.76E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica transversal of 7.76E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | ||||
Glow Wire Ignition Temperature | 800 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 800 °C | IEC 60695-2-13 | 3.0 mm | |||
Heat deflection temperature, 0.45 MPa | 126 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 126 °C | ISO 75/Be | Edgew 120*10*4 sp=100mm | |||
Heat deflection temperature, 1.80 MPa | 111 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 111 °C | ISO 75/Ae | Edgew 120*10*4 sp=100mm | |||
Relative temperature index, electrical | 100 °C Show Supplier Material materials with Relative temperature index, electrical of 100 °C | UL 746B | |||
Relative temperature index, mechanical impact | 85 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 85 °C | UL 746B | |||
Relative temperature index, mechanical strength | 100 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 100 °C | UL 746B | |||
Temperatura de flexión bajo carga | 111 - 126 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 111 - 126 °C | ||||
Temperatura de reblandecimiento Vicat | 132 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 132 °C | ISO 306 | Rate B/50 | |||
Inflamabilidad | UL Recognized, 94-5VA Flame Class Rating: ≥2mm UL 94 <br> UL Recognized, 94V-0 Flame Class Rating: ≥1.5mm UL 94 <br> Radiant Panel Listing: TRUE- UL Tested <br> UV-light, water exposure/immersion: F1- UL 746C <br> Glow Wire Flammability Index, 1.0 mm: 960°C IEC 60695-2-12 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=221170- - <br> Glow Wire Ignitability Temperature, 1.0 mm: 850°C IEC 60695-2-13 |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Constante dieléctrica, 1 MHz | 23.0 °C | 2.7 [-] Show Supplier Material materials with Constante dieléctrica, 1 MHz of 2.7 [-] | ASTM D 150 |
Dielectric constant, 60Hz | 23.0 °C | 2.89 [-] Show Supplier Material materials with Dielectric constant, 60Hz of 2.89 [-] | ASTM D 150 | 50/60 Hz |
Dissipation factor, 1MHz | 23.0 °C | 4.4E-3 [-] Show Supplier Material materials with Dissipation factor, 1MHz of 4.4E-3 [-] | ASTM D 150 |
Dissipation factor, 50Hz | 23.0 °C | 0.02 [-] Show Supplier Material materials with Dissipation factor, 50Hz of 0.02 [-] | ASTM D 150 | 50/60 Hz |
High Amp Arc Ignition | 23.0 °C | 1.5 mm Show Supplier Material materials with High Amp Arc Ignition of 1.5 mm | ≥, UL 746A | PLC 3 |
High Volt Arc Track Rate | 23.0 °C | 3 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 3 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 1.5 mm Show Supplier Material materials with Hot-Wire Ignition of 1.5 mm | ≥, UL 746A | PLC 0 |
Rigidez dieléctrica | 23.0 °C | 17.3 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 17.3 kV/mm | ASTM D 149 | in oil, 3.2 mm |
Sheet resistivity, ROA | 23.0 °C | 1.00E+16 Ω Show Supplier Material materials with Sheet resistivity, ROA of 1.00E+16 Ω | >, ASTM D 257 |
Volume resistivity | 23.0 °C | 1.20E+16 Ω·cm Show Supplier Material materials with Volume resistivity of 1.20E+16 Ω·cm | ASTM D 257 |
Índice de seguimiento comparativo | 23.0 °C | 2 V Show Supplier Material materials with Índice de seguimiento comparativo of 2 V | UL 746A | (UL) {PLC} |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.5 % Show Supplier Material materials with Contracción of 0.5 % | SABIC method | 3.2 mm |
Velocidad de flujo de la masa derretida | 7.6 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 7.6 g/10min | ASTM D 1238 | 280°C/5.0 kgf | |
Velocidad de flujo del volumen derretido | 6 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 6 cm³/10min | ISO 1133 | MVR at 300°C/5.0 kg |
Technological properties
Property | ||
---|---|---|
Application areas | Medical Device, LED Lighting, Laundry Dryer, Meter Gas, Personal Computing, Non-LED Lighting, Oil/Gas, Security/Detection, Respiratory, Small Appliance, Power Manangement, Wireless Communications, Wiring Devices, Wearables, Washing Machine, Building Accessory, Battery Cell, Circuit Protection, Air Conditioning, Document Handling, Displays, Dishwasher, Data Transfer, Electronic Components, Enclosure/Housing/Cover, Enclosures, Individual Equiptment, Hygiene/Personal Care, Furnace/Heater, Food Processor | |
Availability | Americas | |
Processing methods | Shot to Cylinder Size: 30 to 70.0% | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |