General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad relativa | 23.0 °C | 1.1 [-] Show Supplier Material materials with Densidad relativa of 1.1 [-] | ASTM D 792 |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 55 % Show Supplier Material materials with Elongación of 55 % | ASTM D 638 | brk, Type I, 50 mm/min |
Impact strength, Izod notched, ASTM | 23.0 °C | 100 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 100 J/m | ASTM D 256 |
Módulo de flexión | 23.0 °C | 2.5 GPa Show Supplier Material materials with Módulo de flexión of 2.5 GPa | ASTM D 790 | 2.6 mm/min, 100 mm span |
Resistencia a la flexión | 23.0 °C | 100 MPa Show Supplier Material materials with Resistencia a la flexión of 100 MPa | ASTM D 790 | yld, 2.6 mm/min, 100 mm span |
Resistencia a la tracción | 23.0 °C | 65 MPa Show Supplier Material materials with Resistencia a la tracción of 65 MPa | ASTM D 638 | yld, Type I, 50 mm/min |
Resistencia al choque, ensayo Izod entallado | 23.0 °C | 211 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Izod entallado of 211 kJ/m² | ASTM D 256 | notched, 23°C |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 9E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 9E-5 1/K | ASTM E 831 | -40°C to 40°C |
Coeficiente de dilatación térmica transversal | 23.0 °C | 8.5E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica transversal of 8.5E-5 1/K | ASTM E 831 | -40°C to 40°C |
Heat deflection temperature, 0.45 MPa | 195 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 195 °C | ASTM D 648 | 6.4 mm, unannealed | |
Temperatura de flexión bajo carga | 195 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 195 °C |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Dissipation factor, 1MHz | 23.0 °C | 0.02 [-] Show Supplier Material materials with Dissipation factor, 1MHz of 0.02 [-] | ASTM D 150 |
Rigidez dieléctrica | 23.0 °C | 22.4 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 22.4 kV/mm | ASTM D 149 | in oil, 1.6 mm |
Rheological Properties
Property | Value | Comment |
---|---|---|
Velocidad de flujo de la masa derretida | 24 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 24 g/10min | ASTM D 1238 | 280°C/2.16 kgf |
Technological properties
Property | ||
---|---|---|
Application areas | Auto Electrical, Circuit Protection, Auto Aftermarket, Electronic Components, Recreational Vehicle | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Time (Cumulative): 8hrs | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |