General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 23.0 °C | 1.19 g/cm³ Show Supplier Material materials with Densidad of 1.19 g/cm³ | ASTM D 792 |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 122 % Show Supplier Material materials with Elongación of 122 % | ASTM D 638 | brk, Type I, 50 mm/min |
Hardness, Rockwell R | 23.0 °C | 122 [-] Show Supplier Material materials with Hardness, Rockwell R of 122 [-] | ASTM D 785 |
Módulo de flexión | 23.0 °C | 2 GPa Show Supplier Material materials with Módulo de flexión of 2 GPa | ASTM D 790 | 1.3 mm/min, 50 mm span |
Resistencia a la tracción | 23.0 °C | 65 MPa Show Supplier Material materials with Resistencia a la tracción of 65 MPa | ASTM D 638 | yld, Type I, 50 mm/min |
Resistencia al choque, ensayo Izod entallado | 23.0 °C | 640 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Izod entallado of 640 kJ/m² | ASTM D 256 | notched, 23°C |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Conductividad térmica | 23.0 °C | 0.21 W/(m·K) Show Supplier Material materials with Conductividad térmica of 0.21 W/(m·K) | ASTM C177 | ||
Relative temperature index, electrical | 125 °C Show Supplier Material materials with Relative temperature index, electrical of 125 °C | UL 746B | |||
Relative temperature index, mechanical impact | 125 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 125 °C | UL 746B | |||
Relative temperature index, mechanical strength | 125 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 125 °C | UL 746B | |||
Inflamabilidad | UL Recognized, 94V-2 Flame Class Rating: ≥1.5mm UL 94 <br> UL Recognized, 94V-2 Flame Class Rating: ≥1.5mm UL 94 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=220884- - |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Constante dieléctrica, 1 MHz | 23.0 °C | 3 [-] Show Supplier Material materials with Constante dieléctrica, 1 MHz of 3 [-] | ASTM D 150 |
Dissipation factor, 100Hz | 23.0 °C | 0.02 [-] Show Supplier Material materials with Dissipation factor, 100Hz of 0.02 [-] | ASTM D 150 |
High Amp Arc Ignition | 23.0 °C | 1.5 mm Show Supplier Material materials with High Amp Arc Ignition of 1.5 mm | ≥, UL 746A | PLC 4 |
High Volt Arc Track Rate | 23.0 °C | 3 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 3 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 1.5 mm Show Supplier Material materials with Hot-Wire Ignition of 1.5 mm | ≥, UL 746A | PLC 3 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.7 % Show Supplier Material materials with Contracción of 0.7 % | SABIC method | 3.2 mm |
Technological properties
Property | ||
---|---|---|
Application areas | Rear/Signal Lighting, Surgical Devices, Renal and Blood Handling, Monitoring and Imaging, Non-LED Lighting, Motorcycle, Forward Lighting | |
Availability | Europe,Asia,Americas | |
Processing methods | Rear - Zone 1 Temperature: 315 to 340.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |