Property | Temperature | Value | Comment |
---|---|---|---|
Densidad relativa | 23.0 °C | 1.55 [-] Show Supplier Material materials with Densidad relativa of 1.55 [-] | ASTM D 792 |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Impact strength, Izod notched, ASTM | 23.0 °C | 78 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 78 J/m | ASTM D 256 | notched, 23°C |
Módulo de flexión | 23.0 °C | 11.5 GPa Show Supplier Material materials with Módulo de flexión of 11.5 GPa | ASTM D 790 | 6.4 mm |
Resistencia a la flexión | 23.0 °C | 202 MPa Show Supplier Material materials with Resistencia a la flexión of 202 MPa | ASTM D 790 | yield, 6.4 mm |
Resistencia al choque, ensayo Izod entallado | 23.0 °C | 78 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Izod entallado of 78 kJ/m² | ASTM D 256 | notched, 23°C |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 1.32E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.32E-5 1/K | ISO 11359-2 | 23°C to 60°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 8.25E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica transversal of 8.25E-5 1/K | ISO 11359-2 | 23°C to 60°C | ||
Heat deflection temperature, 1.80 MPa | 204 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 204 °C | ASTM D 648 | 6.4 mm, unannealed | |||
Relative temperature index, electrical | 75 °C Show Supplier Material materials with Relative temperature index, electrical of 75 °C | UL 746B | |||
Relative temperature index, mechanical impact | 75 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 75 °C | UL 746B | |||
Relative temperature index, mechanical strength | 75 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 75 °C | UL 746B | |||
Temperatura de flexión bajo carga | 204 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 204 °C | ||||
Inflamabilidad | UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=101283813- - <br> UL Recognized, 94V-0 Flame Class Rating: ≥2mm UL 94 |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Sheet resistivity, ROA | 23.0 °C | 1.30E+6 Ω Show Supplier Material materials with Sheet resistivity, ROA of 1.30E+6 Ω | ASTM D 257 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Personal Computing, ATM/Ticket Machine, Electronic Components | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 120°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |