General
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 7 % Show Supplier Material materials with Elongación of 7 % | ASTM D 638 | yld, Type I, 5 mm/min |
Módulo de flexión | 23.0 °C | 3.5 GPa Show Supplier Material materials with Módulo de flexión of 3.5 GPa | ASTM D 790 | 2.6 mm/min, 100 mm span |
Módulo elástico | 23.0 °C | 3.6 GPa Show Supplier Material materials with Módulo elástico of 3.6 GPa | ASTM D 638 | 5 mm/min |
Resistencia a la flexión | 23.0 °C | 165 MPa Show Supplier Material materials with Resistencia a la flexión of 165 MPa | ASTM D 790 | yld, 2.6 mm/min, 100 mm span |
Resistencia a la tracción | 23.0 °C | 110 MPa Show Supplier Material materials with Resistencia a la tracción of 110 MPa | ASTM D 638 | yld, Type I, 5 mm/min |
Resistencia al choque, ensayo Izod entallado | 23.0 °C | 53 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Izod entallado of 53 kJ/m² | ASTM D 256 | notched, 23°C |
Taber Abrasion | 23.0 °C | 10 mg/1000cy Show Supplier Material materials with Taber Abrasion of 10 mg/1000cy | ASTM D 1044 | CS-17, 1 kg |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 5.58E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 5.58E-5 1/K | ASTM E 831 | -20°C to 150°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 5.4E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica transversal of 5.4E-5 1/K | ASTM E 831 | -20°C to 150°C | ||
Conductividad térmica | 23.0 °C | 0.22 W/(m·K) Show Supplier Material materials with Conductividad térmica of 0.22 W/(m·K) | ASTM C177 | ||
Heat deflection temperature, 0.45 MPa | 210 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 210 °C | ASTM D 648 | 6.4 mm, unannealed | |||
Heat deflection temperature, 1.80 MPa | 201 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 201 °C | ASTM D 648 | 6.4 mm, unannealed | |||
Relative temperature index, electrical | 170 °C Show Supplier Material materials with Relative temperature index, electrical of 170 °C | UL 746B | |||
Relative temperature index, mechanical impact | 170 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 170 °C | UL 746B | |||
Relative temperature index, mechanical strength | 170 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 170 °C | UL 746B | |||
Temperatura de flexión bajo carga | 201 - 210 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 201 - 210 °C | ||||
Temperatura de reblandecimiento Vicat | 218 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 218 °C | ASTM D 1525 | Rate B/50 | |||
Inflamabilidad | UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=101048254- - <br> UL Recognized, 94-5VA Flame Class Rating: ≥3mm UL 94 <br> UL Recognized, 94V-0 Flame Class Rating: ≥0.75mm UL 94 <br> UL Recognized, 94V-2 Flame Class Rating: ≥0.4mm UL 94 <br> UL Recognized, 94V-2 Flame Class Rating: ≥0.4mm UL 94 <br> UV-light, water exposure/immersion: F2- UL 746C <br> NBS Smoke Density, Flaming, Ds 4 min: 0.7- ASTM E 662 |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Factor de disipación | 23.0 °C | 2.5E-3 [-] Show Supplier Material materials with Factor de disipación of 2.5E-3 [-] | ASTM D 150 | 2450 MHz |
High Amp Arc Ignition | 23.0 °C | 3 mm Show Supplier Material materials with High Amp Arc Ignition of 3 mm | ≥, UL 746A | PLC 3 |
High Volt Arc Track Rate | 23.0 °C | 2 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 2 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 3 mm Show Supplier Material materials with Hot-Wire Ignition of 3 mm | ≥, UL 746A | PLC 1 |
Rigidez dieléctrica | 23.0 °C | 19.7 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 19.7 kV/mm | ASTM D 149 | in oil, 3.2 mm |
Volume resistivity | 23.0 °C | 1.00E+17 Ω·cm Show Supplier Material materials with Volume resistivity of 1.00E+17 Ω·cm | ASTM D 257 |
Índice de seguimiento comparativo | 23.0 °C | 4 V Show Supplier Material materials with Índice de seguimiento comparativo of 4 V | UL 746A | (UL) {PLC} |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.5 % Show Supplier Material materials with Contracción of 0.5 % | SABIC method | 3.2 mm |
Technological properties
Property | ||
---|---|---|
Application areas | Additive Plastic, Air Cabin Interiors, Aircraft Seating, Aerospace, Auto Electrical, Circuit Protection, Auto Aftermarket, Audio, Amusement Machine, Animal Testing, Aircraft Exteriors, Defense Vehicles, Displays, Document Handling, Cooking Range, Composite, Commercial Storage/Cookware, Coffee Maker/Espresso Machine, Building Element, Data Management, Data Transfer, Forward Lighting, Food Transportation, Eyeglasses, Furnace/Heater, Fluid Delivery, Food Processor, Fog Lamp, Food Container, Exterior, Electronic Material Handling, Engine Component, Infotainment/Telematic, Industrial Material Handling, Individual Equiptment, Lab Ware and Clinical Diagnostics, Heavy Vehicles, Head Protection, Gear/Bearing/Slider, Enclosures, Enclosure/Housing/Cover, Energy Management, Electronics, Electronic Components, Pharmaceutical Manufacturing, Photo/Video Camera, Pharmaceutical Packaging & Drug Delivery, Power Manangement, Plumbing, Photovoltaic Components, Recreational Vehicle, Refrigerator, Pipe/Fitting, Pump, Rear/Signal Lighting, Rail, Safety Glasses, Respiratory, Security/Detection, Semiconductor, Small Appliance, Sanitary, Servingware, Sensor, Surgical Devices, Personal Care, OLED, Oil/Gas, Non-LED Lighting, Personal Computing, Monitoring and Imaging, Microwave Oven, Meter Gas, Infrastructure, Interior Rail Components, Inverter, Medical Facility Infrastructure, LED Lighting, Medical Device, Wiring Devices, Weapon, Water Treatment/Filtration, Wearables, Wireless Communications, Swimming Pool/Spa, Sunglasses, Surgical Tray, Tray, Vending Machine, Underhood, Washing Machine, Wire & cable, Irrigation | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 150°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |