Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 60 % Show Supplier Material materials with Elongación of 60 % | ISO 527 | break, 50 mm/min |
Módulo de flexión | 23.0 °C | 3.3 GPa Show Supplier Material materials with Módulo de flexión of 3.3 GPa | ISO 178 | 2 mm/min |
Módulo elástico | 23.0 °C | 3.2 GPa Show Supplier Material materials with Módulo elástico of 3.2 GPa | ISO 527 | 1 mm/min |
Resistencia a la flexión | 23.0 °C | 160 MPa Show Supplier Material materials with Resistencia a la flexión of 160 MPa | ISO 178 | yield, 2 mm/min |
Resistencia a la tracción | 23.0 °C | 85 MPa Show Supplier Material materials with Resistencia a la tracción of 85 MPa | ISO 527 | break, 50 mm/min |
Resistencia al choque, ensayo Izod entallado | 23.0 °C | 6 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Izod entallado of 6 kJ/m² | ISO 180/1A | notched 80*10*4, -30°C |
Taber Abrasion | 23.0 °C | 10 mg/1000cy Show Supplier Material materials with Taber Abrasion of 10 mg/1000cy | SABIC method | CS-17, 1 kg |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 5E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 5E-5 1/K | ISO 11359-2 | 23°C to 150°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 5E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica transversal of 5E-5 1/K | ISO 11359-2 | 23°C to 150°C | ||
Conductividad térmica | 23.0 °C | 0.24 W/(m·K) Show Supplier Material materials with Conductividad térmica of 0.24 W/(m·K) | ISO 8302 | ||
Heat deflection temperature, 0.45 MPa | 200 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 200 °C | ISO 75/Be | Edgew 120*10*4 sp=100mm | |||
Heat deflection temperature, 1.80 MPa | 190 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 190 °C | ISO 75/Ae | Edgew 120*10*4 sp=100mm | |||
Relative temperature index, electrical | 170 °C Show Supplier Material materials with Relative temperature index, electrical of 170 °C | UL 746B | |||
Relative temperature index, mechanical impact | 170 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 170 °C | UL 746B | |||
Relative temperature index, mechanical strength | 170 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 170 °C | UL 746B | |||
Temperatura de flexión bajo carga | 190 - 200 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 190 - 200 °C | ||||
Temperatura de reblandecimiento Vicat | 211 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 211 °C | ISO 306 | Rate B/50 | |||
Inflamabilidad | UL Recognized, 94V-0 Flame Class Rating: ≥0.75mm UL 94 <br> UL Recognized, 94V-2 Flame Class Rating: ≥0.4mm UL 94 <br> UL Recognized, 94V-2 Flame Class Rating: ≥0.4mm UL 94 <br> Glow Wire Flammability Index 960°C, passes at: 3.2mm IEC 60695-2-12 <br> Glow Wire Flammability Index 960°C, passes at: 3.2mm IEC 60695-2-12 <br> UL Recognized, 94-5VA Flame Class Rating: ≥3mm UL 94 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=101048254- - <br> UV-light, water exposure/immersion: F2- UL 746C |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Factor de disipación | 23.0 °C | 2.5E-3 [-] Show Supplier Material materials with Factor de disipación of 2.5E-3 [-] | IEC 60250 | 2450 MHz |
High Amp Arc Ignition | 23.0 °C | 3 mm Show Supplier Material materials with High Amp Arc Ignition of 3 mm | ≥, UL 746A | PLC 3 |
High Volt Arc Track Rate | 23.0 °C | 2 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 2 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 3 mm Show Supplier Material materials with Hot-Wire Ignition of 3 mm | ≥, UL 746A | PLC 1 |
Rigidez dieléctrica | 23.0 °C | 16 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 16 kV/mm | IEC 60243-1 | in oil, 3.2 mm, |
Volume resistivity | 23.0 °C | 1.00E+15 Ω·cm Show Supplier Material materials with Volume resistivity of 1.00E+15 Ω·cm | IEC 60093 | |
Índice de seguimiento comparativo | 23.0 °C | 4 V Show Supplier Material materials with Índice de seguimiento comparativo of 4 V | UL 746A | (UL) {PLC} |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.5 % Show Supplier Material materials with Contracción of 0.5 % | SABIC method | 3.2 mm |
Technological properties
Property | ||
---|---|---|
Application areas | Additive Plastic, Air Cabin Interiors, Aircraft Seating, Aerospace, Auto Electrical, Circuit Protection, Auto Aftermarket, Audio, Amusement Machine, Animal Testing, Aircraft Exteriors, Defense Vehicles, Displays, Document Handling, Cooking Range, Composite, Commercial Storage/Cookware, Coffee Maker/Espresso Machine, Building Element, Data Management, Data Transfer, Forward Lighting, Food Transportation, Eyeglasses, Furnace/Heater, Fluid Delivery, Food Processor, Fog Lamp, Food Container, Exterior, Electronic Material Handling, Engine Component, Infotainment/Telematic, Industrial Material Handling, Individual Equiptment, Lab Ware and Clinical Diagnostics, Heavy Vehicles, Head Protection, Gear/Bearing/Slider, Enclosures, Enclosure/Housing/Cover, Energy Management, Electronics, Electronic Components, Pharmaceutical Manufacturing, Photo/Video Camera, Pharmaceutical Packaging & Drug Delivery, Power Manangement, Plumbing, Photovoltaic Components, Recreational Vehicle, Refrigerator, Pipe/Fitting, Pump, Rear/Signal Lighting, Rail, Safety Glasses, Respiratory, Security/Detection, Semiconductor, Small Appliance, Sanitary, Servingware, Sensor, Surgical Devices, Personal Care, OLED, Oil/Gas, Non-LED Lighting, Personal Computing, Monitoring and Imaging, Microwave Oven, Meter Gas, Infrastructure, Interior Rail Components, Inverter, Medical Facility Infrastructure, LED Lighting, Medical Device, Wiring Devices, Weapon, Water Treatment/Filtration, Wearables, Wireless Communications, Swimming Pool/Spa, Sunglasses, Surgical Tray, Tray, Vending Machine, Underhood, Washing Machine, Wire & cable, Irrigation | |
Availability | Europe,Asia,Americas | |
Processing methods | Rear - Zone 1 Temperature: 340 to 395.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |