General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 1.25 % Show Supplier Material materials with Absorción de agua of 1.25 % | ISO 62-1 | (23°C/saturated) |
Densidad | 23.0 °C | 1.27 g/cm³ Show Supplier Material materials with Densidad of 1.27 g/cm³ | ISO 1183 |
Densidad relativa | 23.0 °C | 1.27 [-] Show Supplier Material materials with Densidad relativa of 1.27 [-] | ASTM D 792 | |
Moisture absorption | 23.0 °C | 0.7 % Show Supplier Material materials with Moisture absorption of 0.7 % | ISO 62 | (23°C / 50% RH) |
Índice límite de óxigeno | 23.0 °C | 47 % Show Supplier Material materials with Índice límite de óxigeno of 47 % |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 60 % Show Supplier Material materials with Elongación of 60 % | ISO 527 | break, 5 mm/min |
Impact strength, Izod notched, ASTM | 23.0 °C | 53 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 53 J/m | ASTM D 256 |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 1335 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 1335 J/m | ASTM D 4812 | 23°C |
Módulo de flexión | 23.0 °C | 3.3 GPa Show Supplier Material materials with Módulo de flexión of 3.3 GPa | ISO 178 | 2 mm/min |
Módulo elástico | 23.0 °C | 3.2 GPa Show Supplier Material materials with Módulo elástico of 3.2 GPa | ISO 527 | 1 mm/min |
Resistencia a la flexión | 23.0 °C | 160 MPa Show Supplier Material materials with Resistencia a la flexión of 160 MPa | ISO 178 | yield, 2 mm/min |
Resistencia a la tracción | 23.0 °C | 105 MPa Show Supplier Material materials with Resistencia a la tracción of 105 MPa | ISO 527 | yield, 5 mm/min |
Resistencia al choque, ensayo Charpy entallado | 23.0 °C | 4 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 4 kJ/m² | ISO 179/1eA | V-notch Edgew 80*10*4 sp=62mm, 23°C |
Resistencia al choque, ensayo Izod entallado | 23.0 °C | 6 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Izod entallado of 6 kJ/m² | ISO 180/1A | notched 80*10*4, 23°C |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 5E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 5E-5 1/K | ISO 11359-2 | -40°C to 40°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 5E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica transversal of 5E-5 1/K | ISO 11359-2 | -40°C to 40°C | ||
Heat deflection temperature, 1.80 MPa | 215 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 215 °C | ISO 75/Af | Flatw 80*10*4 sp=64mm | |||
Relative temperature index, electrical | 170 °C Show Supplier Material materials with Relative temperature index, electrical of 170 °C | UL 746B | |||
Relative temperature index, mechanical impact | 170 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 170 °C | UL 746B | |||
Relative temperature index, mechanical strength | 170 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 170 °C | UL 746B | |||
Temperatura de flexión bajo carga | 215 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 215 °C | ||||
Temperatura de reblandecimiento Vicat | 215 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 215 °C | ISO 306 | Rate B/50 | |||
Inflamabilidad | UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=100044765- - <br> UL Recognized, 94-5VA Flame Class Rating: ≥3mm UL 94 <br> UL Recognized, 94V-0 Flame Class Rating: ≥0.75mm UL 94 <br> UL Recognized, 94V-2 Flame Class Rating: ≥0.4mm UL 94 <br> UL Recognized, 94V-2 Flame Class Rating: ≥0.4mm UL 94 <br> NBS Smoke Density, Flaming, Ds 4 min: 0.7- ASTM E 662 |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Dissipation factor, 1kHz | 23.0 °C | 1.3E-3 [-] Show Supplier Material materials with Dissipation factor, 1kHz of 1.3E-3 [-] | ASTM D 150 |
Factor de disipación | 23.0 °C | 2.5E-3 [-] Show Supplier Material materials with Factor de disipación of 2.5E-3 [-] | ASTM D 150 | 2450 MHz |
High Amp Arc Ignition | 23.0 °C | 0.75 mm Show Supplier Material materials with High Amp Arc Ignition of 0.75 mm | ≥, UL 746A | PLC 4 |
High Volt Arc Track Rate | 23.0 °C | 2 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 2 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 0.75 mm Show Supplier Material materials with Hot-Wire Ignition of 0.75 mm | ≥, UL 746A | PLC 2 |
Rigidez dieléctrica | 23.0 °C | 32.7 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 32.7 kV/mm | ASTM D 149 | in air, 1.6 mm |
Volume resistivity | 23.0 °C | 1.00E+17 Ω·cm Show Supplier Material materials with Volume resistivity of 1.00E+17 Ω·cm | ASTM D 257 |
Índice de seguimiento comparativo | 23.0 °C | 4 V Show Supplier Material materials with Índice de seguimiento comparativo of 4 V | UL 746A | (UL) {PLC} |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.5 % Show Supplier Material materials with Contracción of 0.5 % | SABIC method | 3.2 mm |
Velocidad de flujo de la masa derretida | 9 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 9 g/10min | ASTM D 1238 | 337°C/6.6 kgf | |
Velocidad de flujo del volumen derretido | 13 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 13 cm³/10min | ISO 1133 | MVR at 220°C/5.0 kg |
Technological properties
Property | ||
---|---|---|
Application areas | Fluid Delivery, Lab Ware and Clinical Diagnostics, Electronic Components, Animal Testing, Surgical Tray, Pharmaceutical Manufacturing, Pharmaceutical Packaging & Drug Delivery, Surgical Devices, Respiratory, Renal and Blood Handling, Oil/Gas, Medical Facility Infrastructure, Monitoring and Imaging, LED Lighting, Medical Device | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 150°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |