General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.2 % Show Supplier Material materials with Absorción de agua of 0.2 % | ISO 62-1 | (23°C/saturated) |
Densidad | 23.0 °C | 1.24 g/cm³ Show Supplier Material materials with Densidad of 1.24 g/cm³ | ISO 1183 |
Moisture absorption | 23.0 °C | 0.06 % Show Supplier Material materials with Moisture absorption of 0.06 % | ASTM D 570 | (50% RH, Equilibrium) |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 2.6 % Show Supplier Material materials with Elongación of 2.6 % | ISO 527 | break, 5 mm/min |
Hardness, Ball Indentation | 23.0 °C | 220 MPa Show Supplier Material materials with Hardness, Ball Indentation of 220 MPa | ISO 2039-1 | H358/30 |
Impact strength, Izod notched, ASTM | 23.0 °C | 45 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 45 J/m | ASTM D 256 |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 400 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 400 J/m | ASTM D 4812 | 23°C |
Módulo de flexión | 23.0 °C | 6 GPa Show Supplier Material materials with Módulo de flexión of 6 GPa | ISO 178 | 2 mm/min |
Módulo elástico | 23.0 °C | 7.2 GPa Show Supplier Material materials with Módulo elástico of 7.2 GPa | ISO 527 | 1 mm/min |
Resistencia a la flexión | 23.0 °C | 165 MPa Show Supplier Material materials with Resistencia a la flexión of 165 MPa | ISO 178 | break, 2 mm/min |
Resistencia a la tracción | 23.0 °C | 119 MPa Show Supplier Material materials with Resistencia a la tracción of 119 MPa | ISO 527 | break, 5 mm/min |
Resistencia al choque, ensayo Charpy entallado | 23.0 °C | 6 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 6 kJ/m² | ISO 179/2C | 23°C |
Resistencia al choque, ensayo Izod entallado | 23.0 °C | 4 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Izod entallado of 4 kJ/m² | ISO 180/1A | 80*10*4, -30°C |
Resistencia al choque, ensayo Izod no entallado | 23.0 °C | 25 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Izod no entallado of 25 kJ/m² | ISO 180/1U | unnotched 80*10*4, 23°C |
Taber Abrasion | 23.0 °C | 65 mg/1000cy Show Supplier Material materials with Taber Abrasion of 65 mg/1000cy | SABIC method | CS-17, 1 kg |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 3E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 3E-5 1/K | ISO 11359-2 | -40°C to 40°C |
Coeficiente de dilatación térmica transversal | 23.0 °C | 7E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica transversal of 7E-5 1/K | ISO 11359-2 | -40°C to 40°C |
Heat deflection temperature, 0.45 MPa | 139 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 139 °C | ISO 75/Be | Edgew 120*10*4 sp=100mm | |
Heat deflection temperature, 1.80 MPa | 132 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 132 °C | ISO 75/Ae | Edgew 120*10*4 sp=100mm | |
Temperatura de flexión bajo carga | 132 - 139 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 132 - 139 °C | ||
Temperatura de reblandecimiento Vicat | 144 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 144 °C | ISO 306 | Rate B/120 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.2 % Show Supplier Material materials with Contracción of 0.2 % | SABIC method | 3.2 mm |
Contracción transversal | 23.0 °C | 0.3 % Show Supplier Material materials with Contracción transversal of 0.3 % | SABIC method | 3.2 mm |
Velocidad de flujo del volumen derretido | 22 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 22 cm³/10min | ISO 1133 | MVR at 280°C/10.0 kg |
Technological properties
Property | ||
---|---|---|
Application areas | Dishwasher, Fixture Bath/Shower, Food Transportation, Heavy Vehicles, Pump, Pipe/Fitting, Plumbing, Sanitary, Meter Water, Water Treatment/Filtration, Swimming Pool/Spa | |
Availability | Europe,Asia,Americas | |
Processing methods | Hopper Temperature: 60 to 80.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |