General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.9 % Show Supplier Material materials with Absorción de agua of 0.9 % | ISO 62-1 | (23°C/saturated) |
Densidad | 23.0 °C | 1.51 g/cm³ Show Supplier Material materials with Densidad of 1.51 g/cm³ | ISO 1183 |
Moisture absorption | 23.0 °C | 0.5 % Show Supplier Material materials with Moisture absorption of 0.5 % | ISO 62 | (23°C / 50% RH) |
Índice límite de óxigeno | 23.0 °C | 48 % Show Supplier Material materials with Índice límite de óxigeno of 48 % |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 2 % Show Supplier Material materials with Elongación of 2 % | ISO 527 | break, 5 mm/min |
Módulo de flexión | 23.0 °C | 8.5 GPa Show Supplier Material materials with Módulo de flexión of 8.5 GPa | ISO 178 | 2 mm/min |
Módulo elástico | 23.0 °C | 9.5 GPa Show Supplier Material materials with Módulo elástico of 9.5 GPa | ISO 527 | 1 mm/min |
Resistencia a la flexión | 23.0 °C | 225 MPa Show Supplier Material materials with Resistencia a la flexión of 225 MPa | ISO 178 | break, 2 mm/min |
Resistencia a la tracción | 23.0 °C | 165 MPa Show Supplier Material materials with Resistencia a la tracción of 165 MPa | ISO 527 | break, 5 mm/min |
Resistencia al choque, ensayo Charpy entallado | 23.0 °C | 10 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 10 kJ/m² | ISO 179/2C | 23°C |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Ball Pressure Test | nan | IEC 60695-10-2 | 125°C +/- 2°C | |||
Coeficiente de dilatación térmica | 23.0 °C | 2E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 2E-5 1/K | ISO 11359-2 | 23°C to 150°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 6E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica transversal of 6E-5 1/K | ISO 11359-2 | 23°C to 150°C | ||
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | ||||
Glow Wire Ignition Temperature | 900 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 900 °C | IEC 60695-2-13 | 2.0 mm | |||
Heat deflection temperature, 0.45 MPa | 215 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 215 °C | ISO 75/Be | Edgew 120*10*4 sp=100mm | |||
Heat deflection temperature, 1.80 MPa | 210 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 210 °C | ISO 75/Ae | Edgew 120*10*4 sp=100mm | |||
Relative temperature index, electrical | 180 °C Show Supplier Material materials with Relative temperature index, electrical of 180 °C | UL 746B | |||
Relative temperature index, mechanical impact | 170 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 170 °C | UL 746B | |||
Relative temperature index, mechanical strength | 180 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 180 °C | UL 746B | |||
Temperatura de flexión bajo carga | 210 - 215 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 210 - 215 °C | ||||
Temperatura de reblandecimiento Vicat | 220 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 220 °C | ISO 306 | Rate B/120 | |||
Inflamabilidad | UL Recognized, 94-5VA Flame Class Rating: ≥1.2mm UL 94 <br> UL Recognized, 94V-0 Flame Class Rating: ≥0.25mm UL 94 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=221099- - |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Factor de disipación | 23.0 °C | 5.3E-3 [-] Show Supplier Material materials with Factor de disipación of 5.3E-3 [-] | IEC 60250 | 2450 MHz |
High Amp Arc Ignition | 23.0 °C | 3 mm Show Supplier Material materials with High Amp Arc Ignition of 3 mm | ≥, UL 746A | PLC 4 |
High Volt Arc Track Rate | 23.0 °C | 3 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 3 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 3 mm Show Supplier Material materials with Hot-Wire Ignition of 3 mm | ≥, UL 746A | PLC 1 |
Rigidez dieléctrica | 23.0 °C | 15 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 15 kV/mm | IEC 60243-1 | in oil, 3.2 mm, |
Volume resistivity | 23.0 °C | 1.00E+15 Ω·cm Show Supplier Material materials with Volume resistivity of 1.00E+15 Ω·cm | IEC 60093 | |
Índice de seguimiento comparativo | 23.0 °C | 4 V Show Supplier Material materials with Índice de seguimiento comparativo of 4 V | UL 746A | (UL) {PLC} |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.2 % Show Supplier Material materials with Contracción of 0.2 % | SABIC method | on tensile bar |
Velocidad de flujo del volumen derretido | 6 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 6 cm³/10min | ISO 1133 | MVR at 360°C/5.0 kg |
Technological properties
Property | ||
---|---|---|
Application areas | Non-LED Lighting, Electronic Components, Aerospace | |
Availability | Europe,Americas | |
Processing methods | Drying Temperature: 150°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |