General
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 3 % Show Supplier Material materials with Elongación of 3 % | ASTM D 638 | brk, Type I, 5 mm/min |
Módulo de flexión | 23.0 °C | 9 GPa Show Supplier Material materials with Módulo de flexión of 9 GPa | ASTM D 790 | 2.6 mm/min, 100 mm span |
Módulo elástico | 23.0 °C | 9.3 GPa Show Supplier Material materials with Módulo elástico of 9.3 GPa | ASTM D 638 | 5 mm/min |
Resistencia a la flexión | 23.0 °C | 227 MPa Show Supplier Material materials with Resistencia a la flexión of 227 MPa | ASTM D 790 | brk, 2.6 mm/min, 100 mm span |
Resistencia a la tracción | 23.0 °C | 168 MPa Show Supplier Material materials with Resistencia a la tracción of 168 MPa | ASTM D 638 | yld, Type I, 5 mm/min |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 1.98E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.98E-5 1/K | ASTM E 831 | -20°C to 150°C | ||
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | ||||
Glow Wire Ignition Temperature | 900 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 900 °C | IEC 60695-2-13 | 2.0 mm | |||
Heat deflection temperature, 0.45 MPa | 212 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 212 °C | ASTM D 648 | 6.4 mm, unannealed | |||
Heat deflection temperature, 1.80 MPa | 210 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 210 °C | ASTM D 648 | 6.4 mm, unannealed | |||
Relative temperature index, electrical | 180 °C Show Supplier Material materials with Relative temperature index, electrical of 180 °C | UL 746B | |||
Relative temperature index, mechanical impact | 170 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 170 °C | UL 746B | |||
Relative temperature index, mechanical strength | 180 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 180 °C | UL 746B | |||
Temperatura de flexión bajo carga | 210 - 212 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 210 - 212 °C | ||||
Temperatura de reblandecimiento Vicat | 227 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 227 °C | ASTM D 1525 | Rate B/50 | |||
Inflamabilidad | NBS Smoke Density, Flaming, Ds 4 min: 1.6- ASTM E 662 <br> UL Recognized, 94-5VA Flame Class Rating: ≥1.2mm UL 94 <br> UL Recognized, 94V-0 Flame Class Rating: ≥0.25mm UL 94 <br> UV-light, water exposure/immersion: F1- UL 746C <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=221099- - <br> UL Yellow Card Link 2: https://iq.ul.com/ul/cert.aspx?ULID=470961- - |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Factor de disipación | 23.0 °C | 5.3E-3 [-] Show Supplier Material materials with Factor de disipación of 5.3E-3 [-] | ASTM D 150 | 2450 MHz |
High Amp Arc Ignition | 23.0 °C | 1.5 mm Show Supplier Material materials with High Amp Arc Ignition of 1.5 mm | ≥, UL 746A | PLC 3 |
High Volt Arc Track Rate | 23.0 °C | 3 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 3 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 3 mm Show Supplier Material materials with Hot-Wire Ignition of 3 mm | ≥, UL 746A | PLC 1 |
Rigidez dieléctrica | 23.0 °C | 30.3 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 30.3 kV/mm | ASTM D 149 | in oil, 1.6 mm |
Volume resistivity | 23.0 °C | 3.00E+16 Ω·cm Show Supplier Material materials with Volume resistivity of 3.00E+16 Ω·cm | ASTM D 257 |
Índice de seguimiento comparativo | 23.0 °C | 4 V Show Supplier Material materials with Índice de seguimiento comparativo of 4 V | UL 746A | (UL) {PLC} |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.2 % Show Supplier Material materials with Contracción of 0.2 % | SABIC method | on tensile bar |
Technological properties
Property | ||
---|---|---|
Application areas | Electronic Components, Enclosure/Housing/Cover, Electronics, Enclosures, Furnace/Heater, Fluid Delivery, Gear/Bearing/Slider, Heavy Vehicles, Lab Ware and Clinical Diagnostics, Individual Equiptment, Circuit Protection, Auto Electrical, Auto Aftermarket, Aircraft Exteriors, Animal Testing, Air Conditioning, Aerospace, Aircraft Seating, Air Intake System, Air Cabin Interiors, Defense Vehicles, Document Handling, Data Transfer, Data Management, Building/Construction Sheet, Wiring Devices, Weapon, Wireless Communications, Underhood, Vacuum Cleaner, Plumbing, Pharmaceutical Packaging & Drug Delivery, Power Boat, Pipe/Fitting, Pump, Refrigerator, Security/Detection, Semiconductor, Sail Boat, Sanitary, Surgical Devices, Personal Computing, Non-LED Lighting, Oil/Gas, Motorcycle, Navigation Unit, LED Lighting, Medical Device, Meter Gas, Infrastructure, Interior Rail Components | |
Availability | Europe,Asia,Americas | |
Processing methods | Rear - Zone 1 Temperature: 330 to 400.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |