General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.1 % Show Supplier Material materials with Absorción de agua of 0.1 % | ISO 62-1 | (23°C/saturated) |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 1.5 % Show Supplier Material materials with Elongación of 1.5 % | ISO 527 | break, 5 mm/min |
Módulo de flexión | 23.0 °C | 6 GPa Show Supplier Material materials with Módulo de flexión of 6 GPa | ISO 178 | 2 mm/min |
Módulo elástico | 23.0 °C | 8.2 GPa Show Supplier Material materials with Módulo elástico of 8.2 GPa | ISO 527 | 1 mm/min |
Resistencia a la flexión | 23.0 °C | 183 MPa Show Supplier Material materials with Resistencia a la flexión of 183 MPa | ISO 178 |
Resistencia a la tracción | 23.0 °C | 110 MPa Show Supplier Material materials with Resistencia a la tracción of 110 MPa | ISO 527 | break, 50 mm/min |
Resistencia al choque, ensayo Izod no entallado | 23.0 °C | 30 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Izod no entallado of 30 kJ/m² | ISO 180/1U | 80*10*4, 23°C |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 3E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 3E-5 1/K | ISO 11359-2 | 23°C to 80°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 7E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica transversal of 7E-5 1/K | ISO 11359-2 | -40°C to 40°C | ||
Heat deflection temperature, 0.45 MPa | 143 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 143 °C | ISO 75/Bf | Flatw 80*10*4 sp=64mm | |||
Heat deflection temperature, 1.80 MPa | 139 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 139 °C | ISO 75/Af | Flatw 80*10*4 sp=64mm | |||
Relative temperature index, electrical | 65 °C Show Supplier Material materials with Relative temperature index, electrical of 65 °C | UL 746B | |||
Relative temperature index, mechanical impact | 90 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 90 °C | UL 746B | |||
Relative temperature index, mechanical strength | 90 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 90 °C | UL 746B | |||
Temperatura de flexión bajo carga | 139 - 143 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 139 - 143 °C | ||||
Temperatura de reblandecimiento Vicat | 147 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 147 °C | ISO 306 | Rate B/50 | |||
Inflamabilidad | UL Recognized, 94HB Flame Class Rating: 1.5mm UL 94 <br> Glow Wire Flammability Index 850°C, passes at: 3.2mm IEC 60695-2-12 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=236756- - |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Índice de seguimiento comparativo | 23.0 °C | 4 V Show Supplier Material materials with Índice de seguimiento comparativo of 4 V | UL 746A | (UL) {PLC} |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.1 % Show Supplier Material materials with Contracción of 0.1 % | SABIC method | on tensile bar |
Velocidad de flujo del volumen derretido | 7 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 7 cm³/10min | ISO 1133 | MVR at 280°C/10.0 kg |
Technological properties
Property | ||
---|---|---|
Application areas | Auto Aftermarket, Circuit Protection, Building Accessory, Air Conditioning, Displays, Drain Pan, Dishwasher, Document Handling, Building Element, Bottles, Commercial Storage/Cookware, Data Management, Data Transfer, Electronic Components, Energy Management, Enclosure/Housing/Cover, Enclosures, Heavy Vehicles, Hot Water System, Lawn/Garden, Fixture Bath/Shower, Freezer, EV Infrastructure, Water Treatment/Filtration, Wiring Devices, Wireless Communications, Swimming Pool/Spa, Traffic Management, Washing Machine, Vending Machine, LED Lighting, Medical Device, Meter Gas, Ignition System, Medical Facility Infrastructure, Meter Water, Non-LED Lighting, Motorcycle, Personal Computing, Renal and Blood Handling, Semiconductor, Personal Water Craft, Small Appliance, Surgical Devices, Pipe/Fitting, Pump, Recreational Vehicle, Plumbing, Photovoltaic Components, Photo/Video Camera | |
Availability | Europe,Americas | |
Processing methods | Drying Temperature: 100 to 120.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |