LNP THERMOCOMP* MF006SXP is a compound based on Polypropylene resin containing 30% Glass Fiber. Added features of this material include: Chemically Coupled.

Los datos sobre este material han sido proporcionados por Sabic.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValueComment

Densidad

23.0 °C

1.13 g/cm³

Show Supplier Material materials with Densidad of 1.13 g/cm³

ISO 1183

Mecánica

PropertyTemperatureValueComment

Elongación

23.0 °C

2.6 %

Show Supplier Material materials with Elongación of 2.6 %

ISO 527 | yield, 50 mm/min

Módulo de flexión

23.0 °C

8.7 GPa

Show Supplier Material materials with Módulo de flexión of 8.7 GPa

ISO 178

Módulo elástico

23.0 °C

5.7 GPa

Show Supplier Material materials with Módulo elástico of 5.7 GPa

ISO 527 | 1 mm/min

Resistencia a la flexión

23.0 °C

159 MPa

Show Supplier Material materials with Resistencia a la flexión of 159 MPa

ISO 178

Resistencia a la tracción

23.0 °C

81 MPa

Show Supplier Material materials with Resistencia a la tracción of 81 MPa

ISO 527 | yield, 50 mm/min

Resistencia al choque, ensayo Izod entallado

23.0 °C

9 kJ/m²

Show Supplier Material materials with Resistencia al choque, ensayo Izod entallado of 9 kJ/m²

ISO 180/1A | notched 80*10*4, 23°C

Resistencia al choque, ensayo Izod no entallado

23.0 °C

35 kJ/m²

Show Supplier Material materials with Resistencia al choque, ensayo Izod no entallado of 35 kJ/m²

ISO 180/1U | unnotched 80*10*4, 23°C

Aplicaciones térmicas

PropertyTemperatureValueComment

Coeficiente de dilatación térmica

23.0 °C

3.5E-5 1/K

Show Supplier Material materials with Coeficiente de dilatación térmica of 3.5E-5 1/K

ISO 11359-2 | 23°C to 60°C

Coeficiente de dilatación térmica transversal

23.0 °C

1.26E-4 1/K

Show Supplier Material materials with Coeficiente de dilatación térmica transversal of 1.26E-4 1/K

ISO 11359-2 | 23°C to 60°C

Heat deflection temperature, 1.80 MPa

136 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 136 °C

ISO 75/Af | Flatw 80*10*4 sp=64mm

Relative temperature index, electrical

65 °C

Show Supplier Material materials with Relative temperature index, electrical of 65 °C

UL 746B

Relative temperature index, mechanical impact

65 °C

Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C

UL 746B

Relative temperature index, mechanical strength

65 °C

Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C

UL 746B

Temperatura de flexión bajo carga

136 °C

Show Supplier Material materials with Temperatura de flexión bajo carga of 136 °C

Inflamabilidad

UL Recognized, 94HB Flame Class Rating: ≥1mm UL 94 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=101283897- -

Eléctrico

PropertyTemperatureValueComment

High Amp Arc Ignition

23.0 °C

1.5 mm

Show Supplier Material materials with High Amp Arc Ignition of 1.5 mm

≥, UL 746A | PLC 1

High Volt Arc Track Rate

23.0 °C

1 PLC Code

Show Supplier Material materials with High Volt Arc Track Rate of 1 PLC Code

UL 746A | (PLC)

Hot-Wire Ignition

23.0 °C

3 mm

Show Supplier Material materials with Hot-Wire Ignition of 3 mm

≥, UL 746A | PLC 2

Índice de seguimiento comparativo

23.0 °C

0 V

Show Supplier Material materials with Índice de seguimiento comparativo of 0 V

UL 746A | (UL) {PLC}

Technological properties

Property
Availability

Europe,Americas

Processing methods

Back Pressure: 0.2 to 0.3MPa
Front - Zone 3 Temperature: 240 to 250.0°C
Screw Speed: 30 to 60.0rpm
Drying Time: 4hrs
Drying Temperature: 80°C
Mold Temperature: 30 to 50.0°C
Middle - Zone 2 Temperature: 215 to 225.0°C
Rear - Zone 1 Temperature: 195 to 205.0°C
Melt Temperature: 225 to 250.0°C

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.