General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.15 % Show Supplier Material materials with Absorción de agua of 0.15 % | ISO 62-1 | (23°C/saturated) |
Densidad | 23.0 °C | 1.24 g/cm³ Show Supplier Material materials with Densidad of 1.24 g/cm³ | ISO 1183 |
Densidad relativa | 23.0 °C | 1.24 [-] Show Supplier Material materials with Densidad relativa of 1.24 [-] | ASTM D 792 | |
Moisture absorption | 23.0 °C | 0.06 % Show Supplier Material materials with Moisture absorption of 0.06 % | ISO 62 | (23°C / 50% RH) |
Índice límite de óxigeno | 23.0 °C | 23 % Show Supplier Material materials with Índice límite de óxigeno of 23 % |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 2 % Show Supplier Material materials with Elongación of 2 % | ISO 527 | break, 5 mm/min |
Hardness, Ball Indentation | 23.0 °C | 100 MPa Show Supplier Material materials with Hardness, Ball Indentation of 100 MPa | ISO 2039-1 | H358/30 |
Impact strength, Izod notched, ASTM | 23.0 °C | 60 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 60 J/m | ASTM D 256 |
Instrumented Impact, Total Energy | 23.0 °C | 14 J Show Supplier Material materials with Instrumented Impact, Total Energy of 14 J | ASTM D 3763 | 23°C |
Módulo de flexión | 23.0 °C | 4.5 GPa Show Supplier Material materials with Módulo de flexión of 4.5 GPa | ISO 178 | 2 mm/min |
Módulo elástico | 23.0 °C | 6 GPa Show Supplier Material materials with Módulo elástico of 6 GPa | ISO 527 | 1 mm/min |
Resistencia a la flexión | 23.0 °C | 135 MPa Show Supplier Material materials with Resistencia a la flexión of 135 MPa | ISO 178 | break, 2 mm/min |
Resistencia a la tracción | 23.0 °C | 90 MPa Show Supplier Material materials with Resistencia a la tracción of 90 MPa | ISO 527 | yield, 5 mm/min |
Resistencia al choque, ensayo Charpy no entallado | 23.0 °C | 25 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 25 kJ/m² | ISO 179/1eU | Unnotch Edgew 80*10*4 sp=62mm, -30°C |
Resistencia al choque, ensayo Izod entallado | 23.0 °C | 60 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Izod entallado of 60 kJ/m² | ASTM D 256 | notched, 23°C |
Resistencia al choque, ensayo Izod no entallado | 23.0 °C | 25 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Izod no entallado of 25 kJ/m² | ISO 180/1U | unnotched 80*10*4, -30°C |
Taber Abrasion | 23.0 °C | 45 mg/1000cy Show Supplier Material materials with Taber Abrasion of 45 mg/1000cy | SABIC method | CS-17, 1 kg |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Ball Pressure Test | nan | IEC 60695-10-2 | 125°C +/- 2°C | |||
Ball pressure temperature | 165 °C Show Supplier Material materials with Ball pressure temperature of 165 °C | IEC 60695-10-2 | approximate maximum | |||
Coeficiente de dilatación térmica | 23.0 °C | 3E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 3E-5 1/K | ISO 11359-2 | 23°C to 80°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 7E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica transversal of 7E-5 1/K | ISO 11359-2 | 23°C to 80°C | ||
Conductividad térmica | 23.0 °C | 0.26 W/(m·K) Show Supplier Material materials with Conductividad térmica of 0.26 W/(m·K) | ISO 8302 | ||
Heat deflection temperature, 0.45 MPa | 170 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 170 °C | ISO 75/Be | Edgew 120*10*4 sp=100mm | |||
Heat deflection temperature, 1.80 MPa | 160 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 160 °C | ISO 75/Ae | Edgew 120*10*4 sp=100mm | |||
Temperatura de flexión bajo carga | 160 - 170 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 160 - 170 °C | ||||
Temperatura de reblandecimiento Vicat | 180 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 180 °C | ISO 306 | Rate B/120 | |||
Inflamabilidad | Glow Wire Flammability Index 960°C, passes at: 3.2mm IEC 60695-2-12 <br> Glow Wire Flammability Index 960°C, passes at: 3.2mm IEC 60695-2-12 |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Constante dieléctrica, 1 MHz | 23.0 °C | 2.6 [-] Show Supplier Material materials with Constante dieléctrica, 1 MHz of 2.6 [-] | IEC 60250 |
Dielectric constant, 60Hz | 23.0 °C | 2.7 [-] Show Supplier Material materials with Dielectric constant, 60Hz of 2.7 [-] | IEC 60250 | 50/60 Hz |
Dissipation factor, 1MHz | 23.0 °C | 2E-3 [-] Show Supplier Material materials with Dissipation factor, 1MHz of 2E-3 [-] | IEC 60250 |
Dissipation factor, 50Hz | 23.0 °C | 6E-3 [-] Show Supplier Material materials with Dissipation factor, 50Hz of 6E-3 [-] | IEC 60250 | 50/60 Hz |
Rigidez dieléctrica | 23.0 °C | 26 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 26 kV/mm | IEC 60243-1 | in oil, 1.6 mm |
Sheet resistivity, ROA | 23.0 °C | 1.00E+15 Ω Show Supplier Material materials with Sheet resistivity, ROA of 1.00E+15 Ω | >, IEC 60093 |
Volume resistivity | 23.0 °C | 1.00E+15 Ω·cm Show Supplier Material materials with Volume resistivity of 1.00E+15 Ω·cm | IEC 60093 |
Índice de seguimiento comparativo | 23.0 °C | 200 V Show Supplier Material materials with Índice de seguimiento comparativo of 200 V | IEC 60112 | |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.2 % Show Supplier Material materials with Contracción of 0.2 % | SABIC method | on tensile bar |
Velocidad de flujo de la masa derretida | 4.5 g/10min Show Supplier Material materials with Velocidad de flujo de la masa derretida of 4.5 g/10min | ASTM D 1238 | 300°C/5.0 kgf | |
Velocidad de flujo del volumen derretido | 11 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 11 cm³/10min | ISO 1133 | MVR at 300°C/10.0 kg |
Technological properties
Property | ||
---|---|---|
Application areas | Freezer, Electrical, EV/HEV Battery, Industrial Material Handling, Heavy Vehicles, Hot Water System, Electronic Components, Enclosures, Auto Aftermarket, Cooking Range, Washing Machine, Underhood, Wiring Devices, Wireless Communications, Pump, Ignition System, Microwave Oven, Motorcycle, Personal Computing | |
Availability | Europe | |
Processing methods | Mold Temperature: 80 to 120.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |