General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.2 % Show Supplier Material materials with Absorción de agua of 0.2 % | ISO 62-1 | (23°C/saturated) |
Densidad | 23.0 °C | 1.05 g/cm³ Show Supplier Material materials with Densidad of 1.05 g/cm³ | ISO 1183 |
Moisture absorption | 23.0 °C | 0.07 % Show Supplier Material materials with Moisture absorption of 0.07 % | ISO 62 | (23°C / 50% RH) |
Índice límite de óxigeno | 23.0 °C | 19 % Show Supplier Material materials with Índice límite de óxigeno of 19 % |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 30 % Show Supplier Material materials with Elongación of 30 % | ISO 527 | break, 50 mm/min |
Hardness, Ball Indentation | 23.0 °C | 95 MPa Show Supplier Material materials with Hardness, Ball Indentation of 95 MPa | ISO 2039-1 | H358/30 |
Módulo de flexión | 23.0 °C | 2 GPa Show Supplier Material materials with Módulo de flexión of 2 GPa | ISO 178 | 2 mm/min |
Módulo elástico | 23.0 °C | 2.2 GPa Show Supplier Material materials with Módulo elástico of 2.2 GPa | ISO 527 | 1 mm/min |
Resistencia a la flexión | 23.0 °C | 60 MPa Show Supplier Material materials with Resistencia a la flexión of 60 MPa | ISO 178 | yield, 2 mm/min |
Resistencia a la tracción | 23.0 °C | 45 MPa Show Supplier Material materials with Resistencia a la tracción of 45 MPa | ISO 527 | yield, 50 mm/min |
Resistencia al choque, ensayo Charpy entallado | 23.0 °C | 5 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 5 kJ/m² | ISO 179/1eA | V-notch Edgew 80*10*4 sp=62mm, -30°C |
Resistencia al choque, ensayo Izod entallado | 23.0 °C | 11 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Izod entallado of 11 kJ/m² | ISO 180/1A | 80*10*4, 23°C |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Ball Pressure Test | nan | IEC 60695-10-2 | 75°C +/- 2°C | |||
Ball pressure temperature | 115 °C Show Supplier Material materials with Ball pressure temperature of 115 °C | IEC 60695-10-2 | approximate maximum | |||
Coeficiente de dilatación térmica | 23.0 °C | 7E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 7E-5 1/K | ISO 11359-2 | 23°C to 80°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 9E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica transversal of 9E-5 1/K | ISO 11359-2 | 23°C to 80°C | ||
Conductividad térmica | 23.0 °C | 0.22 W/(m·K) Show Supplier Material materials with Conductividad térmica of 0.22 W/(m·K) | ISO 8302 | ||
Heat deflection temperature, 0.45 MPa | 105 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 105 °C | ISO 75/Be | Edgew 120*10*4 sp=100mm | |||
Heat deflection temperature, 1.80 MPa | 95 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 95 °C | ISO 75/Ae | Edgew 120*10*4 sp=100mm | |||
Relative temperature index, electrical | 90 °C Show Supplier Material materials with Relative temperature index, electrical of 90 °C | UL 746B | |||
Relative temperature index, mechanical impact | 85 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 85 °C | UL 746B | |||
Relative temperature index, mechanical strength | 95 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 95 °C | UL 746B | |||
Temperatura de flexión bajo carga | 95 - 105 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 95 - 105 °C | ||||
Temperatura de reblandecimiento Vicat | 115 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 115 °C | ISO 306 | Rate B/120 | |||
Inflamabilidad | Glow Wire Flammability Index 960°C, passes at: 3.2mm IEC 60695-2-12 <br> Glow Wire Flammability Index 960°C, passes at: 3.2mm IEC 60695-2-12 <br> UL Recognized, 94HB Flame Class Rating: ≥1.5mm UL 94 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=236761- - |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Constante dieléctrica, 1 MHz | 23.0 °C | 2.6 [-] Show Supplier Material materials with Constante dieléctrica, 1 MHz of 2.6 [-] | IEC 60250 |
Dielectric constant, 60Hz | 23.0 °C | 2.6 [-] Show Supplier Material materials with Dielectric constant, 60Hz of 2.6 [-] | IEC 60250 | 50/60 Hz |
Dissipation factor, 1MHz | 23.0 °C | 1E-3 [-] Show Supplier Material materials with Dissipation factor, 1MHz of 1E-3 [-] | IEC 60250 |
Dissipation factor, 50Hz | 23.0 °C | 4E-3 [-] Show Supplier Material materials with Dissipation factor, 50Hz of 4E-3 [-] | IEC 60250 | 50/60 Hz |
High Amp Arc Ignition | 23.0 °C | 1.5 mm Show Supplier Material materials with High Amp Arc Ignition of 1.5 mm | ≥, UL 746A | PLC 0 |
High Volt Arc Track Rate | 23.0 °C | 3 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 3 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 1.5 mm Show Supplier Material materials with Hot-Wire Ignition of 1.5 mm | ≥, UL 746A | PLC 3 |
Rigidez dieléctrica | 23.0 °C | 19 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 19 kV/mm | IEC 60243-1 | in oil, 3.2 mm, |
Sheet resistivity, ROA | 23.0 °C | 1.00E+15 Ω Show Supplier Material materials with Sheet resistivity, ROA of 1.00E+15 Ω | >, IEC 60093 |
Volume resistivity | 23.0 °C | 1.00E+15 Ω·cm Show Supplier Material materials with Volume resistivity of 1.00E+15 Ω·cm | IEC 60093 | |
Índice de seguimiento comparativo | 23.0 °C | 2 V Show Supplier Material materials with Índice de seguimiento comparativo of 2 V | UL 746A | (UL) {PLC} |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.5 % Show Supplier Material materials with Contracción of 0.5 % | SABIC method | on tensile bar |
Velocidad de flujo del volumen derretido | 15 cm³/10min Show Supplier Material materials with Velocidad de flujo del volumen derretido of 15 cm³/10min | ISO 1133 | MVR at 280°C/3.8 kg |
Technological properties
Property | ||
---|---|---|
Application areas | Personal Computing, Meter Water, Photovoltaic Components, Plumbing, Pharmaceutical Packaging & Drug Delivery, Refrigerator, Pump, Wheel Cover, Wiring Devices, Swimming Pool/Spa, Bottles, Cladding/Roof, Data Transfer, Circuit Protection, Electronic Components, Energy Management, Enclosures, Freezer, Heavy Vehicles, Lab Ware and Clinical Diagnostics | |
Availability | Europe | |
Processing methods | Nozzle Temperature: 260 to 280.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |