VDM® Alloy 926

Nombres alternativos y comerciales
Cronifer 1925 hMo, Incoloy 926, VDM® Alloy 926
Want to keep this datasheet? Save it now in your required format

Description

1.4529 (X1NiCrMoCuN25-20-7) is an austenitic, special stainless steel that was developed by VDM Metals on the basis of the many times proven VDM® Alloy 904 L (1.4539). Due to its 6.5 % higher molybdenum concentration, VDM® Alloy 926 has a generally improved corrosion resistance and resistance against pitting corrosion and crevice corrosion compared to VDM® Alloy 904 L. This also has a positive effect on the resistance against stress corrosion that is induced by pitting corrosion. It is characterized by the following features and properties:


  • Very good resistance against chloride-induced stress corrosion
  • Increased resistance against stress corrosion in comparison to other austenitic stainless steels
  • Excellent general corrosion resistance when in contact with oxidizing and reducing media
  • Higher strength than VDM® Alloy 904 L (1.4539)
  • Low propensity to form inter-metallic phases
  • Approval for pressure vessels in the temperature range from -196 to 400°C
  • Approval from building supervisory authorities for components and joining elements made of stainless steels, Deutsches Institut für Bautechnik [German Centre of Competence for Construction], September ’98
  • Equivalent Materials

    Los datos sobre este material han sido proporcionados por VDM Metals.

    A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
    Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

    Ashby charts

    See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

    Propiedades

    General

    PropertyTemperatureValue

    Densidad

    23.0 °C

    8.1 g/cm³

    Show Supplier Material materials with Densidad of 8.1 g/cm³

    Mecánica

    PropertyTemperatureValueComment

    Elongación A50

    23.0 °C

    35 %

    Show Supplier Material materials with Elongación A50 of 35 %

    Typical mechanical properties for sheet, plate, strip, rod and bar

    Límite elástico Rp 0,2

    20.0 °C

    300 MPa

    Show Supplier Material materials with Límite elástico Rp 0,2 of 300 MPa

    Typical mechanical properties

    100.0 °C

    230 MPa

    Show Supplier Material materials with Límite elástico Rp 0,2 of 230 MPa

    Typical mechanical properties

    200.0 °C

    190 MPa

    Show Supplier Material materials with Límite elástico Rp 0,2 of 190 MPa

    Typical mechanical properties

    300.0 °C

    170 MPa

    Show Supplier Material materials with Límite elástico Rp 0,2 of 170 MPa

    Typical mechanical properties

    400.0 °C

    160 MPa

    Show Supplier Material materials with Límite elástico Rp 0,2 of 160 MPa

    Typical mechanical properties

    500.0 °C

    120 MPa

    Show Supplier Material materials with Límite elástico Rp 0,2 of 120 MPa

    Typical mechanical properties

    550.0 °C

    105 MPa

    Show Supplier Material materials with Límite elástico Rp 0,2 of 105 MPa

    Typical mechanical properties

    Límite elástico Rp 1,0

    20.0 °C

    340 MPa

    Show Supplier Material materials with Límite elástico Rp 1,0 of 340 MPa

    Typical mechanical properties

    100.0 °C

    270 MPa

    Show Supplier Material materials with Límite elástico Rp 1,0 of 270 MPa

    Typical mechanical properties

    200.0 °C

    225 MPa

    Show Supplier Material materials with Límite elástico Rp 1,0 of 225 MPa

    Typical mechanical properties

    300.0 °C

    205 MPa

    Show Supplier Material materials with Límite elástico Rp 1,0 of 205 MPa

    Typical mechanical properties

    400.0 °C

    190 MPa

    Show Supplier Material materials with Límite elástico Rp 1,0 of 190 MPa

    Typical mechanical properties

    500.0 °C

    150 MPa

    Show Supplier Material materials with Límite elástico Rp 1,0 of 150 MPa

    Typical mechanical properties

    550.0 °C

    135 MPa

    Show Supplier Material materials with Límite elástico Rp 1,0 of 135 MPa

    Typical mechanical properties

    Unlock all property charts

    Módulo elástico

    20.0 °C

    193 GPa

    Show Supplier Material materials with Módulo elástico of 193 GPa

    100.0 °C

    186 GPa

    Show Supplier Material materials with Módulo elástico of 186 GPa

    200.0 °C

    179 GPa

    Show Supplier Material materials with Módulo elástico of 179 GPa

    300.0 °C

    173 GPa

    Show Supplier Material materials with Módulo elástico of 173 GPa

    400.0 °C

    168 GPa

    Show Supplier Material materials with Módulo elástico of 168 GPa

    Unlock all property charts

    Resistencia a la tracción

    23.0 °C

    650 MPa

    Show Supplier Material materials with Resistencia a la tracción of 650 MPa

    Typical mechanical property for sheet, plate, strip, rod and bar

    Resistencia al choque, ensayo Charpy entallado

    -196.0 °C

    1250 kJ/m²

    Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 1250 kJ/m²

    20.0 °C

    1500 kJ/m²

    Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 1500 kJ/m²

    Unlock all property charts

    Aplicaciones térmicas

    PropertyTemperatureValue

    Calor específico

    20.0 °C

    415 J/(kg·K)

    Show Supplier Material materials with Calor específico of 415 J/(kg·K)

    100.0 °C

    435 J/(kg·K)

    Show Supplier Material materials with Calor específico of 435 J/(kg·K)

    200.0 °C

    470 J/(kg·K)

    Show Supplier Material materials with Calor específico of 470 J/(kg·K)

    300.0 °C

    495 J/(kg·K)

    Show Supplier Material materials with Calor específico of 495 J/(kg·K)

    400.0 °C

    510 J/(kg·K)

    Show Supplier Material materials with Calor específico of 510 J/(kg·K)

    Unlock all property charts

    Coeficiente de dilatación térmica

    100.0 °C

    1.5E-5 1/K

    Show Supplier Material materials with Coeficiente de dilatación térmica of 1.5E-5 1/K

    200.0 °C

    1.57E-5 1/K

    Show Supplier Material materials with Coeficiente de dilatación térmica of 1.57E-5 1/K

    300.0 °C

    1.61E-5 1/K

    Show Supplier Material materials with Coeficiente de dilatación térmica of 1.61E-5 1/K

    400.0 °C

    1.64E-5 1/K

    Show Supplier Material materials with Coeficiente de dilatación térmica of 1.64E-5 1/K

    Unlock all property charts

    Conductividad térmica

    20.0 °C

    12 W/(m·K)

    Show Supplier Material materials with Conductividad térmica of 12 W/(m·K)

    100.0 °C

    12.9 W/(m·K)

    Show Supplier Material materials with Conductividad térmica of 12.9 W/(m·K)

    200.0 °C

    14.4 W/(m·K)

    Show Supplier Material materials with Conductividad térmica of 14.4 W/(m·K)

    300.0 °C

    16.5 W/(m·K)

    Show Supplier Material materials with Conductividad térmica of 16.5 W/(m·K)

    400.0 °C

    18.5 W/(m·K)

    Show Supplier Material materials with Conductividad térmica of 18.5 W/(m·K)

    Unlock all property charts

    Temperatura de fusión

    1320 - 1390 °C

    Show Supplier Material materials with Temperatura de fusión of 1320 - 1390 °C

    Eléctrico

    PropertyTemperatureValue

    Resistividad eléctrica

    20.0 °C

    9.6E-7 Ω·m

    Show Supplier Material materials with Resistividad eléctrica of 9.6E-7 Ω·m

    100.0 °C

    9.9E-7 Ω·m

    Show Supplier Material materials with Resistividad eléctrica of 9.9E-7 Ω·m

    200.0 °C

    1.04E-6 Ω·m

    Show Supplier Material materials with Resistividad eléctrica of 1.04E-6 Ω·m

    300.0 °C

    1.08E-6 Ω·m

    Show Supplier Material materials with Resistividad eléctrica of 1.08E-6 Ω·m

    400.0 °C

    1.12E-6 Ω·m

    Show Supplier Material materials with Resistividad eléctrica of 1.12E-6 Ω·m

    Unlock all property charts

    Magnético

    PropertyTemperatureValue

    Permeabilidad magnética relativa

    23.0 °C

    1 [-]

    Show Supplier Material materials with Permeabilidad magnética relativa of 1 [-]

    Chemical properties

    PropertyValueComment

    Azufre

    0.01 %

    Show Supplier Material materials with Azufre of 0.01 %

    max.

    Carbono

    0.02 %

    Show Supplier Material materials with Carbono of 0.02 %

    max.

    Cobre

    0.5 - 1.5 %

    Show Supplier Material materials with Cobre of 0.5 - 1.5 %

    Cromo

    20 - 21 %

    Show Supplier Material materials with Cromo of 20 - 21 %

    Fósforo

    0.03 %

    Show Supplier Material materials with Fósforo of 0.03 %

    max.

    Hierro

    Balance

    Manganeso

    1 %

    Show Supplier Material materials with Manganeso of 1 %

    max.

    Molibdeno

    6 - 7 %

    Show Supplier Material materials with Molibdeno of 6 - 7 %

    Nitrógeno

    0.15 - 0.25 %

    Show Supplier Material materials with Nitrógeno of 0.15 - 0.25 %

    Níquel

    24 - 26 %

    Show Supplier Material materials with Níquel of 24 - 26 %

    Silicona

    0.5 %

    Show Supplier Material materials with Silicona of 0.5 %

    max.

    Technological properties

    Property
    Application areas

    Cronifer 1925 hMo is a polyvalent material which finds application in a wide range of industries: fire fighting systems, seawater filtration systems and process, hydraulic and reinjection piping systems in the offshore industry, bleaching plants in cellulose pulp production, polished rods for corrosive oil wells, flexible pipe systems for the offshore industry, tubing and couplings, wire lines and flowline systems in sour gas production. In sour gas environment the alloy is listed in NACE Standard MR0175 (Sulfide Stress Cracking Resistant Metallic Materials for Oilfield Equipment) as acceptable up to Level V in the annealed or cold-worked condition at a hardness level of 35 HRC max., components for flue-gas desulphurization plants, such as dampers and stacks, evaporators, heat exchangers, filters and mixers used in the manufacture of phosphoric acid, sulphuric acid distribution systems and coolers, concentration and crystallization of salts by evaporation, condensers and piping systems in power stations using polluted cooling waters, containers for transportation of aggressive chemicals, production of organic derivatives with acid chloride catalysts, reverse-osmosis desalination plant. Cronifer 1925 hMo is approved for pressure vessels by VdTÜV from -196 to 400 °C, and by ASME.

    Cold Forming

    The workpieces should be in the annealed condition for cold forming. Due to its high molybdenum concentration, VDM® Alloy 926 has a higher work hardening rate than other austenitic stainless steels. This must be taken into account for the design and selection of forming tools and equipment and during the planning of forming processes. Intermediate annealing is necessary for major cold forming work. For cold forming above 15%, a final solution annealing must be conducted.

    Corrosion properties

    VDM® Alloy 926 is an austenitic, special stainless steel with largely the same chemical composition as VDM® Alloy 904 L, while the nitrogen content was raised to 0.2 % and the molybdenum concentration to about 6.5 %. At the same time, the resistance against stress crack corrosion induced by pitting corrosion is improved. The nitrogen concentration raised to rounded 0.2 % improve the austenite stability and lowers the propensity to form inter-metallic phases. VDM® Alloy 926 is a good pick for media such as diluted sulfuric and phosphorus acids that are contaminated with chlorides, and also for salt concentrations and crystallizations against which the material proves a higher resistance against wear and tear. Due to its good corrosion resistance in seawater, VDM® Alloy 926 is also used for facilities on offshore platforms. The optimal corrosion behavior is only given if the material is used in clean, passivated condition.

    General machinability

    VDM® Alloy 926 is preferably processed in annealed condition. Since the alloy is prone to work hardening, a low cutting speed should be selected with a feed speed that is not too high and the cutting tool should stay engaged at all times. An adequate chip depth is important in order to cut below the previously formed work-hardened zone. An optimal heat dissipation by using large quantities of suitable, preferably aqueous, cold forming lubricants has considerable influence on a stable machining process.

    Heat Treatment

    Solution annealing should take place at temperatures between 1,150 to -1,200°C (2,102 to -2,192°F) and preferably at 1,180°C (2,156°F). The retention time during annealing depends on the semi-finished product thickness. The retention time starts with material temperature equalization; longer times are generally considerably less critical than retention times that are too short. Cooling down should be accelerated with water to achieve optimum properties. Fast air cooling can also be carried out at thicknesses of less than approx. 1.5 mm. The material must be placed in a furnace that has been heated up to the maximum annealing temperature before any heat treatment. For strips as the product form, the heat treatment can be performed in a continuous furnace at a speed and temperature that is adapted to the strip thickness.

    Hot forming

    VDM® Alloy 926 can be hot-formed in a temperature range between 1,200 and 900°C (2,192 and 1,652°F) with subsequent rapid cooling down in water or air. For heating up, workpieces should be placed in a furnace that is already heated up to 1,200 °C (2,192°F). Heat treatment after hot forming is recommended for achieving optimal corrosion behavior.

    Other

    VDM® Alloy 926 has a cubic, face-centered crystal structure.

    Welding

    It must be ensured that work is carried out using targeted heat application and low heat input. The stringer bead technique is recommended. The interpass temperature should not exceed 120°C. In principle, checking of welding parameters is necessary and it is therefore required to observe the section energy that is suitable for the material.