EN 573-3 Grade AW-5083 H12

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMg alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

H12

EN 573-3

Rod, Flat, Tube

20.0 °C

2.64 - 2.66 g/cm³

Show Material materials with Density of 2.64 - 2.66 g/cm³

H12

EN 573-3

Rod, Flat, Tube

20.0 °C

2.64 g/cm³

Show Material materials with Density of 2.64 g/cm³

H12

EN 573-3

Rod, Flat, Tube

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

140.0 MPa

Show Material materials with Bending Fatigue Strength of 140.0 MPa

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Unlock all property charts

Elastic modulus

71.0 GPa

Show Material materials with Elastic modulus of 71.0 GPa

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

-270.0 °C, 20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H12

EN 573-3

Rod, Flat, Tube

20.0 °C

70.0 - 71.0 GPa

Show Material materials with Elastic modulus of 70.0 - 71.0 GPa

H12

EN 573-3

Rod, Flat, Tube

20.0 °C

71.0 GPa

Show Material materials with Elastic modulus of 71.0 GPa

H12

EN 573-3

Rod, Flat, Tube

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H12

EN 573-3

Rod, Flat, Tube

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

H12

EN 573-3

Rod, Flat, Tube

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

H12

EN 573-3

Rod, Flat, Tube

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

H12

EN 573-3

Rod, Flat, Tube

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

H12

EN 573-3

Rod, Flat, Tube

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H12

EN 573-3

Rod, Flat, Tube

Unlock all property charts

Elongation

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H12

EN 573-3

Rod, Tube, Flat

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H12

EN 573-3

Flat

Transverse

Unlock all property charts

Elongation A100

23.0 °C

6 %

Show Material materials with Elongation A100 of 6 %

Elongation A50

20.0 °C

3 - 7 %

Show Material materials with Elongation A50 of 3 - 7 %

23.0 °C

3 - 7 %

Show Material materials with Elongation A50 of 3 - 7 %

Unlock all property charts

Elongation A50, transverse

20.0 °C

3 - 7 %

Show Material materials with Elongation A50, transverse of 3 - 7 %

Elongation, transverse

20.0 °C

6 %

Show Material materials with Elongation, transverse of 6 %

Hardness, Brinell

20.0 °C

90.0 [-]

Show Material materials with Hardness, Brinell of 90.0 [-]

H12

EN 573-3

Rod, Tube

20.0 °C

94.0 [-]

Show Material materials with Hardness, Brinell of 94.0 [-]

H12

EN 573-3

Flat

94.0 [-]

Show Material materials with Hardness, Brinell of 94.0 [-]

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Unlock all property charts

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Unlock all property charts

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H12

EN 573-3

Rod, Flat, Tube

Unlock all property charts

Shear modulus

26.8 GPa

Show Material materials with Shear modulus of 26.8 GPa

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

26.8 - 27.0 GPa

Show Material materials with Shear modulus of 26.8 - 27.0 GPa

H12

EN 573-3

Rod, Flat, Tube

20.0 °C

26.8 GPa

Show Material materials with Shear modulus of 26.8 GPa

H12

EN 573-3

Rod, Flat, Tube

Unlock all property charts

Tensile strength

20.0 °C

280.0 MPa

Show Material materials with Tensile strength of 280.0 MPa

H12

EN 573-3

Rod, Tube

20.0 °C

315.0 - 375.0 MPa

Show Material materials with Tensile strength of 315.0 - 375.0 MPa

H12

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

280.0 MPa

Show Material materials with Tensile strength of 280.0 MPa

H12

EN 573-3, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

315.0 - 375.0 MPa

Show Material materials with Tensile strength of 315.0 - 375.0 MPa

H12

EN 573-3

Flat

Transverse

Unlock all property charts

Tensile strength, transverse

20.0 °C

315 - 375 MPa

Show Material materials with Tensile strength, transverse of 315 - 375 MPa

Yield strength Rp0.2

20.0 °C

200 - 250 MPa

Show Material materials with Yield strength Rp0.2 of 200 - 250 MPa

23.0 °C

200 - 250 MPa

Show Material materials with Yield strength Rp0.2 of 200 - 250 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

250 MPa

Show Material materials with Yield strength Rp0.2, transverse of 250 MPa

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

300 °C, 20 °C, 300.0 °C

2.6e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.6e-05 1/K

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Rod, Flat

200 °C, 20 °C

2.4999999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4999999999999998e-05 1/K

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

100 °C, 20 °C, 100.0 °C

2.42e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.42e-05 1/K

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Rod, Flat

20 °C, -50 °C, -50.0 °C

2.23e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.23e-05 1/K

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Rod, Flat

200.0 °C

2.5e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5e-05 1/K

H12

EN 573-3

Rod, Flat, Tube

Unlock all property charts

Max service temperature

-195.0 - 50.0 °C

Show Material materials with Max service temperature of -195.0 - 50.0 °C

H12

EN 573-3

Rod, Flat, Tube

Long

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Max service temperature, long

-195 - 50 °C

Show Material materials with Max service temperature, long of -195 - 50 °C

Melting point

574.0 - 638.0 °C

Show Material materials with Melting point of 574.0 - 638.0 °C

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H12

EN 573-3

Rod, Flat, Tube

20.0 °C

899.0 - 900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 899.0 - 900.0 J/(kg·K)

H12

EN 573-3

Rod, Flat, Tube

20.0 °C

899.0 J/(kg·K)

Show Material materials with Specific heat capacity of 899.0 J/(kg·K)

H12

EN 573-3

Rod, Flat, Tube

Unlock all property charts

Thermal conductivity

20.0 °C

110.0 - 140.0 W/(m·K)

Show Material materials with Thermal conductivity of 110.0 - 140.0 W/(m·K)

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Rod, Flat

20.0 °C

117.0 - 140.0 W/(m·K)

Show Material materials with Thermal conductivity of 117.0 - 140.0 W/(m·K)

H12

EN 573-3

Rod, Flat, Tube

20.0 °C

110.0 - 117.0 W/(m·K)

Show Material materials with Thermal conductivity of 110.0 - 117.0 W/(m·K)

H12

EN 573-3

Rod, Flat, Tube

20.0 °C

117.0 W/(m·K)

Show Material materials with Thermal conductivity of 117.0 W/(m·K)

H12

EN 573-3

Rod, Flat, Tube

Unlock all property charts

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

16000000.0 - 19000000.0 S/m

Show Material materials with Electrical conductivity of 16000000.0 - 19000000.0 S/m

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Rod, Flat

Unlock all property charts

Electrical resistivity

5.26e-08 - 6.25e-08 Ω·m

Show Material materials with Electrical resistivity of 5.26e-08 - 6.25e-08 Ω·m

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

6e-08 Ω·m

Show Material materials with Electrical resistivity of 6e-08 Ω·m

H12

EN 573-3

Rod, Flat, Tube

20.0 °C

5.2e-08 - 6e-08 Ω·m

Show Material materials with Electrical resistivity of 5.2e-08 - 6e-08 Ω·m

H12

EN 573-3

Rod, Flat, Tube

20.0 °C

6e-08 - 6.2e-08 Ω·m

Show Material materials with Electrical resistivity of 6e-08 - 6.2e-08 Ω·m

H12

EN 573-3

Rod, Flat, Tube

20.0 °C

5.2e-08 - 6.2e-08 Ω·m

Show Material materials with Electrical resistivity of 5.2e-08 - 6.2e-08 Ω·m

H12

EN 573-3

Rod, Flat, Tube

Unlock all property charts

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.05 - 0.25 %

Show Material materials with Chromium of 0.05 - 0.25 %

H12

EN 573-3, EN 485, EN 754

Rod, Flat, Tube, Strip, Sheet, Plate, Forging, Welded Tube, Bar

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H12

EN 573-3, EN 485, EN 754

Rod, Flat, Tube, Strip, Sheet, Plate, Forging, Welded Tube, Bar

Iron

0.4 %

Show Material materials with Iron of 0.4 %

H12

EN 573-3

Rod, Flat, Tube

0.40 %

Show Material materials with Iron of 0.40 %

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Magnesium

4.0 - 4.9 %

Show Material materials with Magnesium of 4.0 - 4.9 %

H12

EN 573-3, EN 485, EN 754

Rod, Flat, Tube, Strip, Sheet, Plate, Forging, Welded Tube, Bar

Manganese

0.4 - 1.0 %

Show Material materials with Manganese of 0.4 - 1.0 %

H12

EN 573-3, EN 485, EN 754

Rod, Flat, Tube, Strip, Sheet, Plate, Forging, Welded Tube, Bar

Other

each 0.05, total 0.15, Rest Al

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

H12

EN 573-3, EN 485, EN 754

Rod, Flat, Tube, Strip, Sheet, Plate, Forging, Welded Tube, Bar

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

H12

EN 573-3, EN 485, EN 754

Rod, Flat, Tube, Strip, Sheet, Plate, Forging, Welded Tube, Bar

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

H12

EN 573-3, EN 485, EN 754

Rod, Flat, Tube, Strip, Sheet, Plate, Forging, Welded Tube, Bar

Technological properties

Property
Anodizing

decorative: sufficient, Protective: good

Brazing

hard brazing (with flux/ without flux): poor / poor, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Seawater: very good, weathering: very good

Workability