EN 573-3 Grade AW-7020 T6

Want to keep this datasheet? Save it now in your required format

Description

Age-hardenable AlZn alloy. The alloy is not food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.77 g/cm³

Show Material materials with Density of 2.77 g/cm³

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

20.0 °C

2.77 g/cm³

Show Material materials with Density of 2.77 g/cm³

T6

EN 573-3

Profile, Rod, Flat, Plate, Tube, Sheet

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

135.0 MPa

Show Material materials with Bending Fatigue Strength of 135.0 MPa

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

Bending angle 90°

3.5 °/t

Show Material materials with Bending angle 90° of 3.5 °/t

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

4.0 °/t

Show Material materials with Bending angle 90° of 4.0 °/t

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

5.5 °/t

Show Material materials with Bending angle 90° of 5.5 °/t

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

8.0 °/t

Show Material materials with Bending angle 90° of 8.0 °/t

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

20.0 °C

68.0 - 70.0 GPa

Show Material materials with Elastic modulus of 68.0 - 70.0 GPa

T6

EN 573-3

Profile, Rod, Flat, Plate, Tube, Sheet

Elongation

3.0 %

Show Material materials with Elongation of 3.0 %

T6

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Tube

A50

4.0 %

Show Material materials with Elongation of 4.0 %

T6

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Tube

A50

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

A100

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3, EN 1386

Strip, Sheet, Plate, Rod, Tube

A50

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

A100

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

A50

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

A100

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

A50

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3, EN 1386, EN 485

Strip, Sheet, Plate, Rod, Tube

A100

9.0 %

Show Material materials with Elongation of 9.0 %

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

A100

10.0 %

Show Material materials with Elongation of 10.0 %

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

A50

10.0 %

Show Material materials with Elongation of 10.0 %

T6

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

A100

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

T6

EN 573-3

Plate

A50

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

T6

EN 573-3

Plate

A50

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3

Sheet

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3

Flat

Transverse

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3

Plate

A50

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3

Sheet

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3

Flat

Transverse

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3

Flat

A50

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3

Sheet

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3

Flat

A50 Transverse

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3

Flat

Transverse

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3

Profile, Rod, Tube, Plate, Flat

A50

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3

Plate, Sheet

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3

Flat

A50 Transverse

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3

Flat

Transverse

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

T6

EN 573-3

Flat

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

T6

EN 573-3

Flat

Transverse

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

T6

EN 573-3

Flat

A50

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

T6

EN 573-3

Profile, Rod, Tube

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

T6

EN 573-3

Flat

A50 Transverse

Hardness, Brinell

98.0 [-]

Show Material materials with Hardness, Brinell of 98.0 [-]

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

101.0 [-]

Show Material materials with Hardness, Brinell of 101.0 [-]

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

104.0 [-]

Show Material materials with Hardness, Brinell of 104.0 [-]

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

20.0 °C

98.0 - 104.0 [-]

Show Material materials with Hardness, Brinell of 98.0 - 104.0 [-]

T6

EN 573-3

Flat

20.0 °C

98.0 - 101.0 [-]

Show Material materials with Hardness, Brinell of 98.0 - 101.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

98.0 [-]

Show Material materials with Hardness, Brinell of 98.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

101.0 - 104.0 [-]

Show Material materials with Hardness, Brinell of 101.0 - 104.0 [-]

T6

EN 573-3

Flat

20.0 °C

101.0 [-]

Show Material materials with Hardness, Brinell of 101.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

104.0 [-]

Show Material materials with Hardness, Brinell of 104.0 [-]

T6

EN 573-3

Flat

20.0 °C

110.0 [-]

Show Material materials with Hardness, Brinell of 110.0 [-]

T6

EN 573-3

Profile, Rod, Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 7000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 7000 Series Aluminium

Shear modulus

26.4 GPa

Show Material materials with Shear modulus of 26.4 GPa

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

20.0 °C

25.0 - 27.0 GPa

Show Material materials with Shear modulus of 25.0 - 27.0 GPa

T6

EN 573-3

Profile, Rod, Flat, Plate, Tube, Sheet

Tensile strength

330.0 MPa

Show Material materials with Tensile strength of 330.0 MPa

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

340.0 MPa

Show Material materials with Tensile strength of 340.0 MPa

T6

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube

350.0 MPa

Show Material materials with Tensile strength of 350.0 MPa

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

20.0 °C

330.0 MPa

Show Material materials with Tensile strength of 330.0 MPa

T6

EN 573-3

Sheet

20.0 °C

330.0 MPa

Show Material materials with Tensile strength of 330.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

340.0 MPa

Show Material materials with Tensile strength of 340.0 MPa

T6

EN 573-3

Rod, Sheet

20.0 °C

340.0 MPa

Show Material materials with Tensile strength of 340.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

350.0 MPa

Show Material materials with Tensile strength of 350.0 MPa

T6

EN 573-3

Profile, Rod, Tube, Plate, Flat

20.0 °C

350.0 MPa

Show Material materials with Tensile strength of 350.0 MPa

T6

EN 573-3

Flat

Transverse

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

-50 °C

2.14e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.14e-05 1/K

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube, Profile, Flat

-50.0 °C

2.14e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.14e-05 1/K

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube, Profile, Flat

20 °C

2.14e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.14e-05 1/K

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube, Profile, Flat

20 °C

2.31e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.31e-05 1/K

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube, Profile, Flat

20 °C

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube, Profile, Flat

20 °C

2.4999999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4999999999999998e-05 1/K

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

100 °C

2.31e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.31e-05 1/K

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube, Profile, Flat

100.0 °C

2.31e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.31e-05 1/K

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube, Profile, Flat

200 °C

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube, Profile, Flat

200.0 °C

2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube, Profile, Flat

300 °C

2.4999999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4999999999999998e-05 1/K

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

300.0 °C

2.5e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5e-05 1/K

T6

EN 573-3

Profile, Rod, Flat, Plate, Tube, Sheet

Melting point

600.0 - 650.0 °C

Show Material materials with Melting point of 600.0 - 650.0 °C

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

Specific heat capacity

875.0 J/(kg·K)

Show Material materials with Specific heat capacity of 875.0 J/(kg·K)

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

20.0 °C

875.0 J/(kg·K)

Show Material materials with Specific heat capacity of 875.0 J/(kg·K)

T6

EN 573-3

Profile, Rod, Flat, Plate, Tube, Sheet

Thermal conductivity

20.0 °C

130.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 - 160.0 W/(m·K)

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Profile, Rod, Flat, Plate, Tube, Sheet, Strip

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

19000000.0 - 23000000.0 S/m

Show Material materials with Electrical conductivity of 19000000.0 - 23000000.0 S/m

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Profile, Rod, Flat, Plate, Tube, Sheet, Strip

Electrical resistivity

4.35e-08 - 5.26e-08 Ω·m

Show Material materials with Electrical resistivity of 4.35e-08 - 5.26e-08 Ω·m

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 - 0.35 %

Show Material materials with Chromium of 0.1 - 0.35 %

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Profile, Rod, Flat, Plate, Tube, Sheet, Strip

Copper

0.2 %

Show Material materials with Copper of 0.2 %

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Profile, Rod, Flat, Plate, Tube, Sheet, Strip

Iron

0.4 %

Show Material materials with Iron of 0.4 %

T6

EN 573-3

Profile, Rod, Flat, Plate, Tube, Sheet

0.40 %

Show Material materials with Iron of 0.40 %

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

Magnesium

1.0 - 1.4 %

Show Material materials with Magnesium of 1.0 - 1.4 %

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Profile, Rod, Flat, Plate, Tube, Sheet, Strip

Manganese

0.05 - 0.5 %

Show Material materials with Manganese of 0.05 - 0.5 %

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Profile, Rod, Flat, Plate, Tube, Sheet, Strip

Silicon

0.35 %

Show Material materials with Silicon of 0.35 %

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Profile, Rod, Flat, Plate, Tube, Sheet, Strip

Zinc

4.0 - 5.0 %

Show Material materials with Zinc of 4.0 - 5.0 %

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Profile, Rod, Flat, Plate, Tube, Sheet, Strip

Zirconium

0.08 - 0.2 %

Show Material materials with Zirconium of 0.08 - 0.2 %

T6

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Profile, Rod, Flat, Plate, Tube, Sheet, Strip

Technological properties

Property
Anodizing

decorative: acceptable, Protective: good

Brazing

hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable

Corrosion properties

Seawater: sufficient, weathering: acceptable

Workability

Bending / Spinning (cold): good (O) / acceptable (O), Impact extrusion (cold): acceptable (O), Deep drawing / upsetting (Condition) good (O) / good (O)