EN 573-3 Grade AW-7022 T6

Want to keep this datasheet? Save it now in your required format

Description

Age-hardenable AlZn alloy. The alloy is not food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.78 g/cm³

Show Material materials with Density of 2.78 g/cm³

T6

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

20.0 °C

2.78 g/cm³

Show Material materials with Density of 2.78 g/cm³

T6

EN 573-3

Profile, Rod, Flat, Tube, Sheet

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

T6

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

20.0 °C

72.0 GPa

Show Material materials with Elastic modulus of 72.0 GPa

T6

EN 573-3

Profile, Rod, Flat, Tube, Sheet

Elongation

3.0 %

Show Material materials with Elongation of 3.0 %

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

A100

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3, EN 755

Strip, Sheet, Plate, Rod, Tube

A50

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

A100

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3, EN 754

Strip, Sheet, Plate, Rod, Tube

A50

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube

A100

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Rod, Tube

A50

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Rod, Tube

A100

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

T6

EN 573-3

Sheet

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

T6

EN 573-3

Flat

Transverse

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3

Profile, Rod, Tube

A50

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3

Sheet

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

T6

EN 573-3

Flat

Transverse

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T6

EN 573-3

Rod, Tube

A50

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3

Profile, Tube, Rod, Sheet

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T6

EN 573-3

Flat

Transverse

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3

Flat

A50

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3

Rod, Tube, Flat

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3

Flat

A50 Transverse

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T6

EN 573-3

Flat

Transverse

Hardness, Brinell

121.0 [-]

Show Material materials with Hardness, Brinell of 121.0 [-]

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

127.0 [-]

Show Material materials with Hardness, Brinell of 127.0 [-]

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

133.0 [-]

Show Material materials with Hardness, Brinell of 133.0 [-]

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

20.0 °C

121.0 - 133.0 [-]

Show Material materials with Hardness, Brinell of 121.0 - 133.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

121.0 - 127.0 [-]

Show Material materials with Hardness, Brinell of 121.0 - 127.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

121.0 [-]

Show Material materials with Hardness, Brinell of 121.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

127.0 - 133.0 [-]

Show Material materials with Hardness, Brinell of 127.0 - 133.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

127.0 [-]

Show Material materials with Hardness, Brinell of 127.0 [-]

T6

EN 573-3

Flat, Sheet

20.0 °C

133.0 [-]

Show Material materials with Hardness, Brinell of 133.0 [-]

T6

EN 573-3

Profile, Rod, Tube, Flat, Sheet

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 7000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 7000 Series Aluminium

Shear modulus

20.0 °C

27.5 GPa

Show Material materials with Shear modulus of 27.5 GPa

T6

EN 573-3

Profile, Rod, Flat, Tube, Sheet

Tensile strength

410.0 MPa

Show Material materials with Tensile strength of 410.0 MPa

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

430.0 MPa

Show Material materials with Tensile strength of 430.0 MPa

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

450.0 MPa

Show Material materials with Tensile strength of 450.0 MPa

T6

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube

460.0 MPa

Show Material materials with Tensile strength of 460.0 MPa

T6

EN 573-3, EN 754

Strip, Sheet, Plate, Rod, Tube

470.0 MPa

Show Material materials with Tensile strength of 470.0 MPa

T6

EN 573-3, EN 755

Strip, Sheet, Plate, Rod, Tube

490.0 MPa

Show Material materials with Tensile strength of 490.0 MPa

T6

EN 573-3, EN 755

Strip, Sheet, Plate, Rod, Tube

20.0 °C

410.0 MPa

Show Material materials with Tensile strength of 410.0 MPa

T6

EN 573-3

Sheet

20.0 °C

410.0 MPa

Show Material materials with Tensile strength of 410.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

430.0 MPa

Show Material materials with Tensile strength of 430.0 MPa

T6

EN 573-3

Sheet

20.0 °C

430.0 MPa

Show Material materials with Tensile strength of 430.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

450.0 MPa

Show Material materials with Tensile strength of 450.0 MPa

T6

EN 573-3

Sheet, Flat

20.0 °C

450.0 MPa

Show Material materials with Tensile strength of 450.0 MPa

T6

EN 573-3

Flat

Transverse

20.0 °C

460.0 MPa

Show Material materials with Tensile strength of 460.0 MPa

T6

EN 573-3

Rod, Tube

20.0 °C

470.0 MPa

Show Material materials with Tensile strength of 470.0 MPa

T6

EN 573-3

Rod

20.0 °C

490.0 MPa

Show Material materials with Tensile strength of 490.0 MPa

T6

EN 573-3

Profile, Rod, Tube

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

T6

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

100 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

T6

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

Melting point

480.0 - 640.0 °C

Show Material materials with Melting point of 480.0 - 640.0 °C

T6

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

Specific heat capacity

795.0 - 1050.0 J/(kg·K)

Show Material materials with Specific heat capacity of 795.0 - 1050.0 J/(kg·K)

Typical for Wrought 7000 Series Aluminium

Thermal conductivity

20.0 °C

130.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 - 160.0 W/(m·K)

T6

EN 573-3, EN 485, EN 754, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

19000000.0 - 23000000.0 S/m

Show Material materials with Electrical conductivity of 19000000.0 - 23000000.0 S/m

T6

EN 573-3, EN 485, EN 754, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate

Electrical resistivity

4.35e-08 - 5.26e-08 Ω·m

Show Material materials with Electrical resistivity of 4.35e-08 - 5.26e-08 Ω·m

T6

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 - 0.3 %

Show Material materials with Chromium of 0.1 - 0.3 %

T6

EN 573-3, EN 485, EN 754, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate

Copper

0.5 - 1.0 %

Show Material materials with Copper of 0.5 - 1.0 %

T6

EN 573-3, EN 485, EN 754, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate

Iron

0.5 %

Show Material materials with Iron of 0.5 %

T6

EN 573-3

Profile, Rod, Flat, Tube, Sheet

0.50 %

Show Material materials with Iron of 0.50 %

T6

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Rod, Tube

Magnesium

2.6 - 3.7 %

Show Material materials with Magnesium of 2.6 - 3.7 %

T6

EN 573-3, EN 485, EN 754, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate

Manganese

0.1 - 0.4 %

Show Material materials with Manganese of 0.1 - 0.4 %

T6

EN 573-3, EN 485, EN 754, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate

Silicon

0.5 %

Show Material materials with Silicon of 0.5 %

T6

EN 573-3, EN 485, EN 754, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate

Zinc

4.3 - 5.2 %

Show Material materials with Zinc of 4.3 - 5.2 %

T6

EN 573-3, EN 485, EN 754, EN 755

Profile, Rod, Flat, Tube, Sheet, Strip, Plate

Technological properties

Property
Anodizing

decorative: not suitable, Protective: good

Brazing

hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: not suitable, soft brazing with flux: not suitable

Corrosion properties

Seawater: poor, weathering: sufficient

Workability

Bending / Spinning (cold): poor (O) / not suitable, Impact extrusion (cold): not suitable, Deep drawing / upsetting (Condition) not suitable / not suitable