EN 573-3 Grade AW-2024 O3

Want to keep this datasheet? Save it now in your required format

Description

Aluminum EN AW-2024, known for its use in aircraft industry, is an alloy that offers excellent strength. When in the annealed condition it is readily formed and has good machinability. Though it has a relatively low level of corrosion resistance, it can be machined to a high finish.

Related Standards

Equivalent Materials

This material data has been provided by AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.77 g/cm³

Show Material materials with Density of 2.77 g/cm³

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Mechanical

PropertyValueConditionRelated StandardsShapeComment

Elastic modulus

73.0 GPa

Show Material materials with Elastic modulus of 73.0 GPa

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 2000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 2000 Series Aluminium

Shear modulus

27.4 GPa

Show Material materials with Shear modulus of 27.4 GPa

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Tensile strength

180.0 - 240.0 MPa

Show Material materials with Tensile strength of 180.0 - 240.0 MPa

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

-50 °C

2.11e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.11e-05 1/K

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C

2.11e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.11e-05 1/K

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C

2.2899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2899999999999998e-05 1/K

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C

2.4699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

100 °C

2.2899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.2899999999999998e-05 1/K

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

100 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

200 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

300 °C

2.4699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Melting point

505.0 - 640.0 °C

Show Material materials with Melting point of 505.0 - 640.0 °C

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

505.0 - 635.0 °C

Show Material materials with Melting point of 505.0 - 635.0 °C

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Specific heat capacity

875.0 J/(kg·K)

Show Material materials with Specific heat capacity of 875.0 J/(kg·K)

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Thermal conductivity

121.0 - 193.0 W/(m·K)

Show Material materials with Thermal conductivity of 121.0 - 193.0 W/(m·K)

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

130.0 - 150.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 - 150.0 W/(m·K)

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Electrical

PropertyValueConditionRelated StandardsShape

Electrical conductivity

17000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 17000000.0 - 29000000.0 S/m

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

18000000.0 - 21000000.0 S/m

Show Material materials with Electrical conductivity of 18000000.0 - 21000000.0 S/m

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Electrical resistivity

3.45e-08 - 5.88e-08 Ω·m

Show Material materials with Electrical resistivity of 3.45e-08 - 5.88e-08 Ω·m

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

4.76e-08 - 5.56e-08 Ω·m

Show Material materials with Electrical resistivity of 4.76e-08 - 5.56e-08 Ω·m

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Copper

3.8 - 4.9 %

Show Material materials with Copper of 3.8 - 4.9 %

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Iron

0.50 %

Show Material materials with Iron of 0.50 %

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Magnesium

1.2 - 1.8 %

Show Material materials with Magnesium of 1.2 - 1.8 %

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Manganese

0.3 - 0.9 %

Show Material materials with Manganese of 0.3 - 0.9 %

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Silicon

0.5 %

Show Material materials with Silicon of 0.5 %

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

O3

EN 573-3, EN 1715-3

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Technological properties

Property
Anodizing

decorative: not suitable, Protective: good

Brazing

hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable

Corrosion properties

Seawater: poor, weathering: poor

Workability

Bending / Spinning (cold): sufficient (O) / acceptable (O), Impact extrusion (cold): acceptable (O), Deep drawing / upsetting (Condition) acceptable (O) / sufficient (O)