General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.72 g/cm³ Show Material materials with Density of 2.72 g/cm³ | H24 | EN 573-3, EN 1592, EN 485, EN 546 | Strip, Sheet, Plate, Welded Tube | |
20.0 °C | 2.72 g/cm³ Show Material materials with Density of 2.72 g/cm³ | H24 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Foil, Flat, Seamless Tube, Coil, Sheet |
Dimension
Property | Value | Condition | Related Standards | Thickness | Shape |
---|---|---|---|---|---|
Thickness | 0.04 mm Show Material materials with Thickness of 0.04 mm | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | 0.04 mm | Coil, Sheet |
1.5 mm Show Material materials with Thickness of 1.5 mm | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | 1.5 mm | Coil, Sheet |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending angle 180° | 1.5 °/t Show Material materials with Bending angle 180° of 1.5 °/t | H24 | EN 573-3, EN 485 | Strip, Sheet, Plate, Welded Tube | ||
1.5 °/t Show Material materials with Bending angle 180° of 1.5 °/t | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Coil, Sheet | |||
Bending angle 90° | 0.5 °/t Show Material materials with Bending angle 90° of 0.5 °/t | H24 | EN 573-3, EN 485 | Strip, Sheet, Plate, Welded Tube | ||
0.5 °/t Show Material materials with Bending angle 90° of 0.5 °/t | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Coil, Sheet | |||
1.0 °/t Show Material materials with Bending angle 90° of 1.0 °/t | H24 | EN 573-3, EN 485 | Strip, Sheet, Plate, Welded Tube | |||
1.5 °/t Show Material materials with Bending angle 90° of 1.5 °/t | H24 | EN 573-3, EN 485 | Strip, Sheet, Plate, Welded Tube | |||
Elastic modulus | 69.0 GPa Show Material materials with Elastic modulus of 69.0 GPa | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Coil, Sheet | ||
70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | H24 | EN 573-3, EN 1592, EN 485, EN 546 | Strip, Sheet, Plate, Welded Tube | |||
Elongation | 1.0 - 3.0 % Show Material materials with Elongation of 1.0 - 3.0 % | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Coil, Sheet | A50 | |
3.0 % Show Material materials with Elongation of 3.0 % | H24 | EN 573-3, EN 546 | Strip, Sheet, Plate, Welded Tube | A50 | ||
4.0 % Show Material materials with Elongation of 4.0 % | H24 | EN 573-3, EN 485, EN 546 | Strip, Sheet, Plate, Welded Tube | A50 | ||
7.0 % Show Material materials with Elongation of 7.0 % | H24 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Welded Tube | A100 | ||
20.0 °C | 3.0 % Show Material materials with Elongation of 3.0 % | H24 | EN 573-3 | Foil | A100 | |
20.0 °C | 3.0 % Show Material materials with Elongation of 3.0 % | H24 | EN 573-3 | Foil | A50 | |
20.0 °C | 4.0 % Show Material materials with Elongation of 4.0 % | H24 | EN 573-3 | Foil | A100 | |
20.0 °C | 4.0 % Show Material materials with Elongation of 4.0 % | H24 | EN 573-3 | Flat, Foil | A50 | |
20.0 °C | 4.0 % Show Material materials with Elongation of 4.0 % | H24 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 7.0 % Show Material materials with Elongation of 7.0 % | H24 | EN 573-3 | Seamless Tube | ||
Hardness, Brinell | 52.0 [-] Show Material materials with Hardness, Brinell of 52.0 [-] | H24 | EN 573-3, EN 485 | Strip, Sheet, Plate, Welded Tube | ||
20.0 °C | 52.0 [-] Show Material materials with Hardness, Brinell of 52.0 [-] | H24 | EN 573-3 | Flat | ||
Hardness, HBW | 53 [-] Show Material materials with Hardness, HBW of 53 [-] | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Coil, Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Shear modulus | 26.0 GPa Show Material materials with Shear modulus of 26.0 GPa | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Coil, Sheet | ||
20.0 °C | 26.5 GPa Show Material materials with Shear modulus of 26.5 GPa | H24 | EN 573-3 | Foil, Flat, Seamless Tube | ||
Tensile strength | 125.0 - 225.0 MPa Show Material materials with Tensile strength of 125.0 - 225.0 MPa | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Coil, Sheet | ||
200.0 MPa Show Material materials with Tensile strength of 200.0 MPa | H24 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Welded Tube | |||
20.0 °C | 170.0 - 215.0 MPa Show Material materials with Tensile strength of 170.0 - 215.0 MPa | H24 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Welded Tube | ||
20.0 °C | 170.0 - 215.0 MPa Show Material materials with Tensile strength of 170.0 - 215.0 MPa | H24 | EN 573-3 | Flat | Transverse | |
20.0 °C | 180.0 - 225.0 MPa Show Material materials with Tensile strength of 180.0 - 225.0 MPa | H24 | EN 573-3, EN 546 | Foil, Strip, Sheet, Plate, Welded Tube | ||
20.0 °C | 200.0 MPa Show Material materials with Tensile strength of 200.0 MPa | H24 | EN 573-3 | Seamless Tube | ||
Yield strength | 45 MPa Show Material materials with Yield strength of 45 MPa | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Coil, Sheet | ||
130.0 MPa Show Material materials with Yield strength of 130.0 MPa | H24 | EN 573-3, EN 485 | Strip, Sheet, Plate, Welded Tube | RP02 | ||
175.0 MPa Show Material materials with Yield strength of 175.0 MPa | H24 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Welded Tube | RP02 | ||
20.0 °C | 130.0 MPa Show Material materials with Yield strength of 130.0 MPa | H24 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 130.0 MPa Show Material materials with Yield strength of 130.0 MPa | H24 | EN 573-3 | Flat | RP02 | |
20.0 °C | 175.0 MPa Show Material materials with Yield strength of 175.0 MPa | H24 | EN 573-3 | Seamless Tube | RP02 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K | H24 | EN 573-3, EN 1592, EN 485, EN 546 | Strip, Sheet, Plate, Welded Tube | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K | H24 | EN 573-3, EN 1592, EN 485, EN 546 | Strip, Sheet, Plate, Welded Tube | ||
100 °C | 0.000024 1/K Show Material materials with Coefficient of thermal expansion of 0.000024 1/K | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Coil, Sheet | 20-100°C | |
Melting point | 630.0 - 654.0 °C Show Material materials with Melting point of 630.0 - 654.0 °C | H24 | EN 573-3, EN 1592, EN 485, EN 546 | Strip, Sheet, Plate, Welded Tube | ||
Specific heat capacity | 20.0 °C | 893.0 J/(kg·K) Show Material materials with Specific heat capacity of 893.0 J/(kg·K) | H24 | EN 573-3 | Foil, Flat, Seamless Tube | |
Thermal conductivity | 160.0 - 190.0 W/(m·K) Show Material materials with Thermal conductivity of 160.0 - 190.0 W/(m·K) | H24 | EN 573-3, EN 1592, EN 485, EN 546 | Strip, Sheet, Plate, Welded Tube | ||
172 W/(m·K) Show Material materials with Thermal conductivity of 172 W/(m·K) | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Coil, Sheet | |||
20.0 °C | 200.0 W/(m·K) Show Material materials with Thermal conductivity of 200.0 W/(m·K) | H24 | EN 573-3 | Foil, Flat, Seamless Tube |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 23000000.0 - 25000000.0 S/m Show Material materials with Electrical conductivity of 23000000.0 - 25000000.0 S/m | H24 | EN 573-3, EN 1592, EN 485, EN 546 | Strip, Sheet, Plate, Welded Tube | |
20.0 °C | 28000000.0 S/m Show Material materials with Electrical conductivity of 28000000.0 S/m | H24 | EN 573-3 | Foil, Flat, Seamless Tube | |
Electrical resistivity | 3.7999999999999996e-08 Ω·m Show Material materials with Electrical resistivity of 3.7999999999999996e-08 Ω·m | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Coil, Sheet | |
4e-08 - 4.35e-08 Ω·m Show Material materials with Electrical resistivity of 4e-08 - 4.35e-08 Ω·m | H24 | EN 573-3, EN 1592, EN 485, EN 546 | Strip, Sheet, Plate, Welded Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.1 % Show Material materials with Chromium of 0.1 % | H24 | EN 573-3, EN 1592, EN 485, EN 546 | Foil, Flat, Seamless Tube, Strip, Sheet, Plate, Welded Tube |
0.1 % Show Material materials with Chromium of 0.1 % | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Coil, Sheet | |
Copper | 0.3 % Show Material materials with Copper of 0.3 % | H24 | EN 573-3, EN 1592, EN 485, EN 546 | Foil, Flat, Seamless Tube, Strip, Sheet, Plate, Welded Tube |
0.3 % Show Material materials with Copper of 0.3 % | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Coil, Sheet | |
Iron | 0.7 % Show Material materials with Iron of 0.7 % | H24 | EN 573-3 | Foil, Flat, Seamless Tube |
0.70 % Show Material materials with Iron of 0.70 % | H24 | EN 573-3, EN 1592, EN 485, EN 546 | Strip, Sheet, Plate, Welded Tube | |
0.7 % Show Material materials with Iron of 0.7 % | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Coil, Sheet | |
Magnesium | 0.2 - 0.6 % Show Material materials with Magnesium of 0.2 - 0.6 % | H24 | EN 573-3, EN 1592, EN 485, EN 546, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Foil, Flat, Seamless Tube, Strip, Sheet, Plate, Welded Tube, Coil, Sheet |
Manganese | 1.0 - 1.5 % Show Material materials with Manganese of 1.0 - 1.5 % | H24 | EN 573-3, EN 1592, EN 485, EN 546, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Foil, Flat, Seamless Tube, Strip, Sheet, Plate, Welded Tube, Coil, Sheet |
Silicon | 0.6 % Show Material materials with Silicon of 0.6 % | H24 | EN 573-3, EN 1592, EN 485, EN 546 | Foil, Flat, Seamless Tube, Strip, Sheet, Plate, Welded Tube |
0.6 % Show Material materials with Silicon of 0.6 % | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Coil, Sheet | |
Titanium | 0.1 % Show Material materials with Titanium of 0.1 % | H24 | EN 573-3, EN 1592, EN 485, EN 546 | Foil, Flat, Seamless Tube, Strip, Sheet, Plate, Welded Tube |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H24 | EN 573-3, EN 1592, EN 485, EN 546 | Foil, Flat, Seamless Tube, Strip, Sheet, Plate, Welded Tube |
0.25 % Show Material materials with Zinc of 0.25 % | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541 | Coil, Sheet |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Electronic devices: Housing of devices; Insulation; Cosmetics: Cosmetics pieces | |
Brazing | Good | |
Corrosion properties | Seawater: very good, weathering: very good | |
Welding | Good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (O) / acceptable (H12) |