EN 573-3 Grade AW-3103 H224

Want to keep this datasheet? Save it now in your required format

Related Standards

Equivalent Materials

This material data has been provided by AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.73 g/cm³

Show Material materials with Density of 2.73 g/cm³

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Mechanical

PropertyValueConditionRelated StandardsShapeComment

Bending angle 90°

1.25 °/t

Show Material materials with Bending angle 90° of 1.25 °/t

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

2.5 °/t

Show Material materials with Bending angle 90° of 2.5 °/t

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Elastic modulus

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 3000 Series Aluminium

Shear modulus

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Tensile strength

115.0 - 175.0 MPa

Show Material materials with Tensile strength of 115.0 - 175.0 MPa

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Melting point

645.0 - 655.0 °C

Show Material materials with Melting point of 645.0 - 655.0 °C

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Specific heat capacity

893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 893.0 J/(kg·K)

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Thermal conductivity

160.0 - 200.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 200.0 W/(m·K)

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Electrical

PropertyValueConditionRelated StandardsShape

Electrical conductivity

22000000.0 - 28000000.0 S/m

Show Material materials with Electrical conductivity of 22000000.0 - 28000000.0 S/m

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Electrical resistivity

3.57e-08 - 4.55e-08 Ω·m

Show Material materials with Electrical resistivity of 3.57e-08 - 4.55e-08 Ω·m

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Iron

0.70 %

Show Material materials with Iron of 0.70 %

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Magnesium

0.3 %

Show Material materials with Magnesium of 0.3 %

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Manganese

0.9 - 1.5 %

Show Material materials with Manganese of 0.9 - 1.5 %

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Silicon

0.5 %

Show Material materials with Silicon of 0.5 %

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

H224

EN 573-3, EN 1386

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Brazing

hard brazing (with flux/ without flux): very good to good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Seawater: good, weathering: very good

Workability

Bending / Spinning (cold): very good / very good, Impact extrusion (cold): good, Deep drawing / upsetting (Condition) very good (O) / very good (H12)