Properties

General

Density

ρ

2.73 g/cm³ at 20 °C

Dimension

Dimensions

Durchmesser

Thickness

t

0.06 - 4 mm

Mechanical

Bending angle 90°

θ90

1.5 - 3 °/t at 20 °C

Show 3000 Series materials with Bending angle 90° of 1.5 - 3 °/t at 20 °C

Elastic modulus

E

70 GPa at -270 °C

Show 3000 Series materials with Elastic modulus of 70 GPa at -270 °C

Hide chart

Elongation

A

30 % at -196 °C

Show 3000 Series materials with Elongation of 30 % at -196 °C

Unlock all property charts

Elongation A100

A100

1 - 3 % at 20 °C

Show 3000 Series materials with Elongation A100 of 1 - 3 % at 20 °C

Elongation A50

A50

1 - 2 % at 20 °C

Show 3000 Series materials with Elongation A50 of 1 - 2 % at 20 °C

Elongation A50, transverse

A50,trans

1 - 2 % at 20 °C

Show 3000 Series materials with Elongation A50, transverse of 1 - 2 % at 20 °C

Hardness, Brinell

HB

55 - 58 [-] at 20 °C

Show 3000 Series materials with Hardness, Brinell of 55 - 58 [-] at 20 °C

Hardness, HBW

HBW

62 [-] at 20 °C

Show 3000 Series materials with Hardness, HBW of 62 [-] at 20 °C

Plane-Strain Fracture Toughnes

KIC

22 - 35 MPa·√m at 20 °C

Show 3000 Series materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m at 20 °C

Typical for Wrought 3000 Series Aluminium

Poisson's ratio

ν

0.33 [-] at 20 °C

Show 3000 Series materials with Poisson's ratio of 0.33 [-] at 20 °C

Shear modulus

G

24 - 26.5 GPa at 20 °C

Show 3000 Series materials with Shear modulus of 24 - 26.5 GPa at 20 °C

Tensile strength

Rm

298 MPa at -196 °C

Show 3000 Series materials with Tensile strength of 298 MPa at -196 °C

Unlock all property charts

Tensile strength, transverse

Rm,trans

185 MPa at 20 °C

Show 3000 Series materials with Tensile strength, transverse of 185 MPa at 20 °C

Yield strength

YS

165 MPa at 20 °C

Show 3000 Series materials with Yield strength of 165 MPa at 20 °C

Yield strength Rp0.2

Rp0.2

232 MPa at -196 °C

Show 3000 Series materials with Yield strength Rp0.2 of 232 MPa at -196 °C

Unlock all property charts

Yield strength Rp0.2, transverse

Rp0.2,trans

165 MPa at 20 °C

Show 3000 Series materials with Yield strength Rp0.2, transverse of 165 MPa at 20 °C

Thermal

Coefficient of thermal expansion

α

2.35E-5 1/K at 20 °C

20-100°C

Unlock all property charts

Melting point

Tm

645 - 655 °C

Specific heat capacity

cp

892 - 893 J/(kg·K) at 20 °C

Thermal conductivity

λ

160 - 200 W/(m·K) at 20 °C

Electrical

Electrical conductivity

σel

2.20E+7 - 2.90E+7 S/m at 20 °C

Electrical resistivity

ρel

3.4E-8 - 4.55E-8 Ω·m at 20 °C

Chemical properties

Element

Weight %

Comment

Other

-

Ti + Zr < 0.10, each 0.05, total 0.15, Rest Al

Mn

0.9 - 1.5 %

Fe

0.7 %

Si

0.5 %

Mg

0.3 %

More

Technological properties

Anodizing

Very Good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing Quality; Lithography; Heat exchangers: Fins, Heat exchangers; Tubes: Flexible tube, Pipes; Cosmetics: Cosmetics pieces; Semi-rigid and corrugated: Smooth wall; Components: Automotive fins, Heat exchangers

Brazing

Excellent

Corrosion properties

Very Good

Welding

Very Good

Workability

Very Good

This material data has been provided by Aludium,WIAM,AluKey.