AlMg3Si-F casting

Want to keep this datasheet? Save it now in your required format

This material data has been provided by Alu Key.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

Electrical

PropertyTemperatureValue

Electrical conductivity

20.0 °C

1.50E+7 S/m

Show Material materials with Electrical conductivity of 1.50E+7 S/m

Electrical resistivity

20.0 °C

4.35E-8 - 6.67E-8 Ω·m

Show Material materials with Electrical resistivity of 4.35E-8 - 6.67E-8 Ω·m

General

PropertyTemperatureValue

Density

20.0 °C

2.66 g/cm³

Show Material materials with Density of 2.66 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

70 GPa

Show Material materials with Elastic modulus of 70 GPa

Thermal

PropertyTemperatureValue

Melting point

560 - 650 °C

Show Material materials with Melting point of 560 - 650 °C

Thermal conductivity

20.0 °C

115 - 160 W/(m·K)

Show Material materials with Thermal conductivity of 115 - 160 W/(m·K)

Chemical properties

PropertyValue

Copper

0.02 %

Show Material materials with Copper of 0.02 %

Iron

0.15 %

Show Material materials with Iron of 0.15 %

Magnesium

3.5 %

Show Material materials with Magnesium of 3.5 %

Manganese

0.4 %

Show Material materials with Manganese of 0.4 %

Silicon

1.3 %

Show Material materials with Silicon of 1.3 %

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %