EN 573-3 Grade AW-5005A H26

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMg alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

20.0 °C

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H26

EN 573-3

Flat

20.0 °C

2.69 - 2.7 g/cm³

Show Material materials with Density of 2.69 - 2.7 g/cm³

H26

EN 573-3

Flat

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H26

EN 573-3

Flat

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 90°

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

2.5 °/t

Show Material materials with Bending angle 90° of 2.5 °/t

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

Elastic modulus

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

20.0 °C

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

H26

EN 573-3

Flat

Hardness, Brinell

52.0 [-]

Show Material materials with Hardness, Brinell of 52.0 [-]

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

20.0 °C

52.0 [-]

Show Material materials with Hardness, Brinell of 52.0 [-]

H26

EN 573-3

Flat

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H26

EN 573-3

Flat

Shear modulus

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

20.0 °C

25.0 - 26.1 GPa

Show Material materials with Shear modulus of 25.0 - 26.1 GPa

H26

EN 573-3

Flat

20.0 °C

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

H26

EN 573-3

Flat

Tensile strength

20.0 °C

165.0 - 205.0 MPa

Show Material materials with Tensile strength of 165.0 - 205.0 MPa

H26

EN 573-3

Flat

Transverse

20.0 °C

165.0 - 205.0 MPa

Show Material materials with Tensile strength of 165.0 - 205.0 MPa

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar, Flat

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50 °C

2.18e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar, Flat

-50.0 °C

2.18e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar, Flat

20 °C

2.18e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar, Flat

20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar, Flat

20 °C

2.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar, Flat

20 °C

2.55e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.55e-05 1/K

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar, Flat

100 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar, Flat

100.0 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar, Flat

200 °C

2.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar, Flat

200.0 °C

2.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar, Flat

300 °C

2.55e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.55e-05 1/K

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar, Flat

300.0 °C

2.55e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.55e-05 1/K

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar, Flat

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

630.0 - 650.0 °C

Show Material materials with Melting point of 630.0 - 650.0 °C

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

Specific heat capacity

20.0 °C

879.0 J/(kg·K)

Show Material materials with Specific heat capacity of 879.0 J/(kg·K)

H26

EN 573-3

Flat

20.0 °C

879.0 - 899.0 J/(kg·K)

Show Material materials with Specific heat capacity of 879.0 - 899.0 J/(kg·K)

H26

EN 573-3

Flat

20.0 °C

899.0 J/(kg·K)

Show Material materials with Specific heat capacity of 899.0 J/(kg·K)

H26

EN 573-3

Flat

Thermal conductivity

20.0 °C

160.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 220.0 W/(m·K)

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar, Flat

20.0 °C

160.0 - 201.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 201.0 W/(m·K)

H26

EN 573-3

Flat

20.0 °C

201.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 201.0 - 220.0 W/(m·K)

H26

EN 573-3

Flat

20.0 °C

201.0 W/(m·K)

Show Material materials with Thermal conductivity of 201.0 W/(m·K)

H26

EN 573-3

Flat

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

23000000.0 - 31000000.0 S/m

Show Material materials with Electrical conductivity of 23000000.0 - 31000000.0 S/m

H26

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Tube, Bar

Electrical resistivity

3.23e-08 - 4.35e-08 Ω·m

Show Material materials with Electrical resistivity of 3.23e-08 - 4.35e-08 Ω·m

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

20.0 °C

3.3e-08 Ω·m

Show Material materials with Electrical resistivity of 3.3e-08 Ω·m

H26

EN 573-3

Flat

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

H26

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Tube, Bar

Copper

0.05 %

Show Material materials with Copper of 0.05 %

H26

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Tube, Bar

Iron

0.45 %

Show Material materials with Iron of 0.45 %

H26

EN 573-3

Flat

0.45 %

Show Material materials with Iron of 0.45 %

H26

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

Magnesium

0.7 - 1.1 %

Show Material materials with Magnesium of 0.7 - 1.1 %

H26

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Tube, Bar

Manganese

0.15 %

Show Material materials with Manganese of 0.15 %

H26

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Tube, Bar

Silicon

0.3 %

Show Material materials with Silicon of 0.3 %

H26

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Tube, Bar

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

H26

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Tube, Bar

Technological properties

Property
Anodizing

decorative: gut (EQ: sehr gut), Protective: very good

Brazing

hard brazing (with flux/ without flux): sufficient - poor / sufficient, friction soldering: good, soft brazing with flux: acceptable

Corrosion properties

Seawater: good, weathering: very good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (H12)