Naturally hard AlMg alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H112

EN 573-3

Profile, Rod, Tube

20.0 °C

2.69 - 2.7 g/cm³

Show Material materials with Density of 2.69 - 2.7 g/cm³

H112

EN 573-3

Profile, Rod, Tube

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H112

EN 573-3

Profile, Rod, Tube

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

H112

EN 573-3

Profile, Rod, Tube

Elongation

16.0 %

Show Material materials with Elongation of 16.0 %

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

A50

18.0 %

Show Material materials with Elongation of 18.0 %

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

A100

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

H112

EN 573-3

Profile, Tube, Rod

A50

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

H112

EN 573-3

Profile, Tube, Rod

Hardness, Brinell

20.0 °C

30.0 [-]

Show Material materials with Hardness, Brinell of 30.0 [-]

H112

EN 573-3

Profile, Tube, Rod

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H112

EN 573-3

Profile, Rod, Tube

Shear modulus

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

25.0 - 26.1 GPa

Show Material materials with Shear modulus of 25.0 - 26.1 GPa

H112

EN 573-3

Profile, Rod, Tube

20.0 °C

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

H112

EN 573-3

Profile, Rod, Tube

Tensile strength

100.0 MPa

Show Material materials with Tensile strength of 100.0 MPa

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

100.0 MPa

Show Material materials with Tensile strength of 100.0 MPa

H112

EN 573-3

Profile, Tube, Rod

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50 °C

2.18e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod

-50.0 °C

2.18e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod

20 °C

2.18e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod

20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod

20 °C

2.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod

20 °C

2.55e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.55e-05 1/K

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod

100 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod

100.0 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod

200 °C

2.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod

200.0 °C

2.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod

300 °C

2.55e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.55e-05 1/K

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod

300.0 °C

2.55e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.55e-05 1/K

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

630.0 - 650.0 °C

Show Material materials with Melting point of 630.0 - 650.0 °C

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

Specific heat capacity

20.0 °C

879.0 J/(kg·K)

Show Material materials with Specific heat capacity of 879.0 J/(kg·K)

H112

EN 573-3

Profile, Rod, Tube

20.0 °C

879.0 - 899.0 J/(kg·K)

Show Material materials with Specific heat capacity of 879.0 - 899.0 J/(kg·K)

H112

EN 573-3

Profile, Rod, Tube

20.0 °C

899.0 J/(kg·K)

Show Material materials with Specific heat capacity of 899.0 J/(kg·K)

H112

EN 573-3

Profile, Rod, Tube

Thermal conductivity

20.0 °C

160.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 220.0 W/(m·K)

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod

20.0 °C

160.0 - 201.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 201.0 W/(m·K)

H112

EN 573-3

Profile, Rod, Tube

20.0 °C

201.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 201.0 - 220.0 W/(m·K)

H112

EN 573-3

Profile, Rod, Tube

20.0 °C

201.0 W/(m·K)

Show Material materials with Thermal conductivity of 201.0 W/(m·K)

H112

EN 573-3

Profile, Rod, Tube

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

23000000.0 - 31000000.0 S/m

Show Material materials with Electrical conductivity of 23000000.0 - 31000000.0 S/m

H112

EN 573-3, EN 755

Profile, Rod, Tube, Strip, Sheet, Plate, Bar

Electrical resistivity

3.23e-08 - 4.35e-08 Ω·m

Show Material materials with Electrical resistivity of 3.23e-08 - 4.35e-08 Ω·m

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

3.3e-08 Ω·m

Show Material materials with Electrical resistivity of 3.3e-08 Ω·m

H112

EN 573-3

Profile, Rod, Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

H112

EN 573-3, EN 755

Profile, Rod, Tube, Strip, Sheet, Plate, Bar

Copper

0.05 %

Show Material materials with Copper of 0.05 %

H112

EN 573-3, EN 755

Profile, Rod, Tube, Strip, Sheet, Plate, Bar

Iron

0.45 %

Show Material materials with Iron of 0.45 %

H112

EN 573-3

Profile, Rod, Tube

0.45 %

Show Material materials with Iron of 0.45 %

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

Magnesium

0.7 - 1.1 %

Show Material materials with Magnesium of 0.7 - 1.1 %

H112

EN 573-3, EN 755

Profile, Rod, Tube, Strip, Sheet, Plate, Bar

Manganese

0.15 %

Show Material materials with Manganese of 0.15 %

H112

EN 573-3, EN 755

Profile, Rod, Tube, Strip, Sheet, Plate, Bar

Silicon

0.3 %

Show Material materials with Silicon of 0.3 %

H112

EN 573-3, EN 755

Profile, Rod, Tube, Strip, Sheet, Plate, Bar

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

H112

EN 573-3, EN 755

Profile, Rod, Tube, Strip, Sheet, Plate, Bar

Technological properties

Property
Anodizing

decorative: gut (EQ: sehr gut), Protective: very good

Brazing

hard brazing (with flux/ without flux): sufficient - poor / sufficient, friction soldering: good, soft brazing with flux: acceptable

Corrosion properties

Seawater: good, weathering: very good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (H12)